Pretreatment liquid and method for producing electromagnetic steel sheet with insulating coating
By adding acetic acid to the pretreatment liquid, the problem of short pretreatment time in the prior art was solved, and an electromagnetic steel plate with insulated film with excellent adhesion and low iron loss was achieved. Ensures the stability of magnetic properties.
Patent Information
- Application Number
- CN202280093927.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art has challenges in reducing iron loss of electromagnetic steel plates, especially while thinning thickness and improving productivity, short pretreatment time leads to insufficient removal of impurity elements, resulting in deterioration of magnetic properties and increasing iron loss.
A specific amount of acetic acid is added to the pretreatment solution containing inorganic acids such as phosphoric acid, and is used to pretreat the forsteril film to ensure that impurities can be fully removed even if the pretreatment time is short, forming excellent adhesion and low iron loss insulating film.
The insulated film electromagnetic steel plate with excellent adhesion and low iron loss is achieved, so that impurity elements are prevented from intruding into the steel plate again and the deterioration of magnetic characteristics is suppressed.
Smart Images

Figure BDA0005051940920000131 
Figure BDA0005051940920000141 
Figure BDA0005051940920000151
Abstract
Description
Technical Field
[0001] The present invention relates to a pretreatment liquid and a method for producing an electromagnetic steel sheet with an insulating coating. Background Art
[0002] Generally, an electromagnetic steel sheet has a coating on its surface that imparts properties such as insulation, sintering resistance, and rust resistance. For example, a grain-oriented electromagnetic steel sheet has a coating containing forsterite (forsterite coating) formed on the surface of the steel sheet during final finish annealing and an insulating coating formed thereon (Patent Document 1).
[0003] The insulating film used in the grain-oriented electrical steel sheet is formed by applying an insulating film treatment liquid containing a salt such as phosphate on a forsterite film and sintering the film at a high temperature.
[0004] The insulating film has a lower thermal expansion coefficient than the steel sheet. Therefore, when the temperature is lowered to room temperature after sintering, tension is applied to the steel sheet by the insulating film, and the iron loss is reduced.
[0005] However, as described above, the forsterite film is formed on the surface of the steel sheet during the final finish annealing, but at this time, impurity elements in the steel sheet may be mixed into the forsterite film. Examples of the impurity elements include sulfur (S) and selenium (Se).
[0006] In this state, when sintering (or planarization annealing serving as sintering) is performed to form an insulating film, the impurity elements penetrate into the steel sheet again from the forsterite film.
[0007] As a result, the obtained electrical steel sheet with an insulating coating may have deteriorated magnetic properties, for example, increased iron loss.
[0008] Therefore, Patent Document 1 describes that a forsterite film is subjected to a pretreatment by phosphoric acid pickling (phosphoric acid pickling pretreatment) before applying an insulating film treatment liquid.
[0009] Patent Document 1 describes that by performing phosphoric acid pickling pretreatment, S as an impurity element mixed in the forsterite film is removed and the reintrusion of S as an impurity element into the steel sheet is suppressed.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Laid-Open No. 09-321486 Summary of the invention
[0013] In recent years, from the perspective of meeting the increasing demand for reducing iron loss, there has been a significant demand for reducing the thickness of steel sheets in order to reduce eddy current loss. Due to the reduction in thickness, the productivity expressed as the amount of production per hour decreases. On the other hand, due to the increase in power demand, the demand for grain-oriented electromagnetic steel sheets continues to increase.
[0014] Therefore, the speed increase of the production line was investigated, but the pre-treatment time was reduced due to the speed increase.
[0015] If the pretreatment time is short, the removal of impurity elements from the forsterite film may be insufficient. In this case, it is not possible to suppress the re-intrusion of impurity elements from the forsterite film into the steel sheet during annealing (or flattening annealing), and the iron loss of the obtained electromagnetic steel sheet with an insulating film becomes high.
[0016] Therefore, increasing the temperature of the pretreatment liquid (pretreatment temperature) has been studied.
[0017] However, in this case, the forsterite film is damaged by the pretreatment liquid, and the adhesion of the forsterite film to the steel sheet is likely to decrease. In this case, the iron loss also increases.
[0018] The present invention has been made in view of the above problems, and an object of the present invention is to obtain an electrical steel sheet with an insulating coating having excellent adhesion of a forsterite coating and low iron loss.
[0019] The present inventors have conducted intensive studies to achieve the above-mentioned object.
[0020] As a result, the inventors have found that by adding a specific amount of acetic acid to a pretreatment solution containing an inorganic acid such as phosphoric acid, impurity elements derived from the forsterite film can be sufficiently removed even if the pretreatment time is short, thereby completing the present invention.
[0021] That is, the present invention provides the following [1] to [6].
[0022] [1] A pretreatment solution for use before applying an insulating coating treatment solution containing at least one salt selected from phosphates, borates and silicates to an electromagnetic steel sheet having a forsterite coating on its surface, the pretreatment solution containing at least one inorganic acid selected from hydrochloric acid, sulfuric acid and phosphoric acid and acetic acid, wherein the content of the acetic acid is 1 to 3000 ppm by mass.
[0023] [2] The pretreatment liquid according to [1] above, wherein the content of the inorganic acid is 0.20% by mass to 30.00% by mass.
[0024] [3] A method for manufacturing an electromagnetic steel sheet with an insulating coating, comprising pretreating an electromagnetic steel sheet having a forsterite coating on its surface using the pretreatment solution described in [1] or [2] above, then applying an insulating coating treatment solution containing at least one salt selected from phosphates, borates and silicates and sintering the resultant to form an insulating coating.
[0025] [4] The method for producing an electrical steel sheet with an insulating coating according to [3] above, wherein the pretreatment is a treatment in which the pretreatment liquid is brought into contact with the forsterite coating.
[0026] [5] The method for producing an electrical steel sheet with an insulating coating according to [4] above, wherein the temperature of the pretreatment liquid is 30° C. to 95° C., and the contact time between the pretreatment liquid and the forsterite coating is 1.0 second to 40 seconds.
[0027] [6] The method for producing an electrical steel sheet with an insulating coating according to any one of [3] to [5] above, wherein the content of the chromium compound in the insulating coating treatment liquid is 1.0 part by mass or less in terms of chromium element relative to 100 parts by mass of the salt.
[0028] According to the present invention, it is possible to obtain an electrical steel sheet with an insulating coating which has excellent adhesion of a forsterite coating and low iron loss. DETAILED DESCRIPTION
[0029] 〈Pretreatment liquid〉
[0030] First, the pretreatment liquid will be described.
[0031] The pretreatment liquid is used before applying the insulating film treatment liquid described later to the electromagnetic steel sheet having the forsterite film on the surface.
[0032] Mineral Acid
[0033] The pretreatment liquid contains at least one inorganic acid selected from the group consisting of hydrochloric acid, sulfuric acid, and phosphoric acid.
[0034] The pretreatment of bringing such a pretreatment liquid into contact with the forsterite film of the electromagnetic steel sheet before applying the insulating film treatment liquid can obtain the following effects.
[0035] First, unnecessary annealing separator (annealing separator remaining after being applied before final finish annealing) is removed.
[0036] Furthermore, the surface of the forsterite film becomes moderately rough, and the wettability with the insulating film treatment liquid applied later is improved, thereby preventing uneven application of the insulating film treatment liquid and liquid repellency.
[0037] The insulating film thus obtained has a uniform and beautiful appearance and also has good insulation properties and tension applied to the steel sheet.
[0038] Furthermore, impurity elements (S, Se, etc.) doped in the forsterite film are removed. As a result, during sintering (or flattening annealing that also serves as sintering) for forming an insulating film, the impurity elements are prevented from entering the steel sheet again. In this way, the deterioration of magnetic properties is suppressed, and an electromagnetic steel sheet with an insulating film having a low iron loss is obtained.
[0039] From the viewpoint of removing impurity elements in the forsterite film, phosphoric acid is preferred as the inorganic acid.
[0040] The content of the inorganic acid in the pretreatment liquid (the total content of hydrochloric acid, sulfuric acid, and phosphoric acid) is preferably 0.20 mass % or more, more preferably 0.50 mass % or more, because impurity elements in the forsterite film can be sufficiently removed in a short time.
[0041] On the other hand, if the content of the inorganic acid is too high, the forsterite film is damaged and the adhesion is easily deteriorated. Therefore, from the reason that the adhesion of the forsterite film is more excellent, the content of the inorganic acid in the pretreatment liquid is preferably 30.00 mass % or less, and more preferably 25.00 mass % or less.
[0042] The content of hydrochloric acid is converted into the content of HCl, the content of sulfuric acid is converted into the content of H2SO4, and the content of phosphoric acid is converted into the content of H3PO4.
[0043] That is, the contents of hydrochloric acid, sulfuric acid, and phosphoric acid in the pretreatment solution are determined by quantifying chloride ions (Cl - ), sulfate ion (SO4 2- ) and phosphate ions (PO4 3- ) and convert it into hydrochloric acid, sulfuric acid and phosphoric acid to find it.
[0044] Acetic acid
[0045] The pretreatment liquid contains acetic acid (CH3COOH) in addition to the inorganic acid. This improves the ability of the inorganic acid to remove impurity elements in the forsterite film.
[0046] The reason for obtaining such an effect is not yet clear, but is presumed as follows.
[0047] The impurity elements (S, Se) exist in the forsterite film in the form of sulfur compounds and / or selenium compounds (hereinafter also referred to as “impurity compounds”).
[0048] Through acetate ion (CH3COO - ) is adsorbed on the surface of the impurity compound, and the dissolution rate of the impurity compound in the inorganic acid is increased.
[0049] At this time, if the content of acetic acid is too low, the amount of acetic acid adsorbed on the impurity compounds is too small, and a sufficient effect cannot be obtained.
[0050] On the other hand, if the content of acetic acid is too high, the amount of acetic acid adsorbed on the impurity compound increases, resulting in steric hindrance, and the dissolution rate of the impurity compound in the inorganic acid decreases, thereby reducing the effect.
[0051] Therefore, the content of acetic acid in the pretreatment liquid is 1 mass ppm or more, preferably 3 mass ppm or more, and more preferably 5 mass ppm or more.
[0052] On the other hand, the content of acetic acid in the pretreatment liquid is 3000 mass ppm or less, preferably 2500 mass ppm or less, and more preferably 2000 mass ppm or less.
[0053] The acetic acid in the pretreatment liquid was quantitatively determined using ion chromatography.
[0054] Ion chromatography was performed under the following conditions.
[0055] Column: Connect two Shodex RSpakKC-G8B (inner diameter 8.0mm, length 50mm) and two Shodex RSpakKC-811 (inner diameter 8.0mm, length 300mm)
[0056] Column temperature: 50℃
[0057] Mobile phase: 3mmol / L perchloric acid
[0058] Reaction solution: Shodex ST3-R (diluted 10 times)
[0059] Flow rate: mobile phase 1.0 mL / min, reaction solution 0.7 mL / min
[0060] Measurement wavelength: 430nm
[0061] Injection volume: 20 μL
[0062] Solvents
[0063] As the solvent of the pretreatment liquid, water is preferred.
[0064] 《Preparation method》
[0065] As a method for preparing the pretreatment liquid, for example, there is a method of preparing the pretreatment liquid by weighing and mixing an inorganic acid and acetic acid as reagents or industrial chemicals of known concentrations and diluting the mixture with water to a desired content.
[0066] 〈Insulation coating treatment liquid〉
[0067] Next, the insulating film processing liquid will be described.
[0068] "Salt"
[0069] The insulating film treatment liquid contains at least one salt selected from phosphates, borates and silicates. Thus, the obtained insulating film has excellent adhesion to the forsterite film.
[0070] The phosphate is preferably a phosphate containing at least one metal element selected from the group consisting of Mg, Ca, Ba, Sr, Zn, Al, and Mn.
[0071] The phosphate may be used alone or in combination of two or more. By using two or more phosphates in combination, the physical property values of the insulating film can be precisely controlled.
[0072] As the phosphate, dihydrogen phosphate (dihydrogen phosphate) is preferred because of its easy availability.
[0073] Examples of the borate include borax (Na2B4O5(OH)4·8H2O) and sodium polyborate.
[0074] Examples of silicates include sodium silicate (Na 3 SiO 3 ) and lithium silicate.
[0075] As the salt, borosilicate, borophosphate, silicophosphate, aluminosilicate, or the like can be used.
[0076] 《Colloidal Silica》
[0077] The insulating film treatment liquid preferably further contains colloidal silica.
[0078] The content of colloidal silica is preferably 20 parts by mass or more, more preferably 50 parts by mass or more, based on the SiO2 solid content conversion relative to 100 parts by mass of salt. If the content of colloidal silica is within this range, the effect of reducing the thermal expansion coefficient of the insulating film becomes greater, and the tension applied to the steel sheet is further increased.
[0079] On the other hand, because the adhesion between the insulating film and the forsterite film is better, the content of colloidal silica is preferably 120 parts by mass or less, and more preferably 100 parts by mass or less, calculated as SiO2 solid content, relative to 100 parts by mass of the salt.
[0080] Chromium compounds
[0081] The insulating film treatment liquid is preferably a so-called chromium-free liquid that does not contain chromium compounds such as chromic anhydride (chromium trioxide), chromate, and dichromate.
[0082] Specifically, the content of the chromium compound is preferably 1.0 part by mass or less, more preferably 0.10 part by mass or less, and even more preferably 0.01 part by mass or less, in terms of chromium element (Cr) relative to 100 parts by mass of the salt.
[0083] Metal Compounds
[0084] The insulating film treatment liquid preferably contains a metal compound (a compound containing a metal element).
[0085] The content of the metal compound is preferably 5.0 parts by mass or more, more preferably 10 parts by mass or more, in terms of metal element conversion, relative to 100 parts by mass of the salt. As a result, the obtained insulating film has good moisture absorption resistance, corrosion resistance, etc., and the tension applied to the steel sheet becomes higher. In the case where the insulating film treatment liquid is chromium-free, these characteristics may be insufficient, so it is more useful.
[0086] On the other hand, the content of the metal compound is preferably 60 parts by mass or less, more preferably 40 parts by mass or less, in terms of metal element conversion, relative to 100 parts by mass of the salt. If the content of the metal compound is within this range, the insulating film treatment liquid can be kept at a low viscosity, so it is easy to obtain an insulating film with uniform film thickness.
[0087] The metal element contained in the metal compound is preferably at least one selected from the group consisting of Ti, Zr, Hf, V, Mg, Zn and Nb because the obtained insulating film has better moisture absorption resistance.
[0088] The metal compound is a compound such as an oxide or a nitride containing these metal elements, and its form is, for example, particles.
[0089] Solvents
[0090] As the solvent of the insulating film treatment liquid, water is preferable.
[0091] 〈Electromagnetic steel sheet having forsterite coating〉
[0092] The electromagnetic steel sheet having a forsterite film is not particularly limited as long as it has a steel sheet and a forsterite film (a film containing forsterite) disposed on the surface of the steel sheet, and one example is a grain-oriented electromagnetic steel sheet.
[0093] 《Composition of Steel》
[0094] First, a preferred chemical composition of steel will be described. Hereinafter, unless otherwise specified, the unit "%" of the content of each element means "mass %".
[0095] (C: 0.0010~0.10%)
[0096] C is useful for generating Goss-oriented grains. In order to exert this effect, the C content is preferably 0.0010% or more.
[0097] On the other hand, if the C content is too high, decarburization may be insufficient even in decarburization annealing. Therefore, the C content is preferably 0.10% or less.
[0098] (Si: 1.0-5.0%)
[0099] Si increases electrical resistance, reduces iron loss, stabilizes the BCC structure of iron, and enables high-temperature heat treatment. Therefore, the Si content is preferably 1.0% or more, and more preferably 2.0% or more.
[0100] On the other hand, if the Si content is too high, cold rolling becomes difficult. Therefore, the Si content is preferably 5.0% or less.
[0101] (Mn: 0.010~1.0%)
[0102] Mn effectively contributes to improving the hot brittleness of steel. Furthermore, when S and Se are mixed, Mn forms precipitates such as MnS and MnSe, and functions as an inhibitor of grain growth. Therefore, the Mn content is preferably 0.010% or more.
[0103] On the other hand, if the Mn content is too high, the particle size of precipitates such as MnSe may become coarse and the function as an inhibitor may be lost. Therefore, the Mn content is preferably 1.0% or less.
[0104] (sol.Al: 0.0030~0.050%)
[0105] Al forms AlN in steel, becomes a dispersed second phase, and functions as an inhibitor. Therefore, the Al content is preferably 0.0030% or more as sol.Al.
[0106] On the other hand, if the Al content is too high, AlN may coarsely precipitate and lose its function as an inhibitor. Therefore, the Al content is preferably 0.050% or less as sol.Al.
[0107] (N: 0.0010~0.020%)
[0108] N forms AlN in the presence of Al. Therefore, the N content is preferably 0.0010% or more.
[0109] On the other hand, if the N content is too high, swelling etc. may occur when the slab is heated. Therefore, the N content is preferably 0.020% or less.
[0110] (at least one of S and Se: 0.0010 to 0.050%)
[0111] S and Se combine with Mn and Cu to form MnSe, MnS, Cu2-xSe, and Cu2-xS, which become dispersed second phases in steel and function as inhibitors. Therefore, the total content of at least one of S and Se is preferably 0.0010% or more.
[0112] On the other hand, if the content of S and Se is too high, not only will the solid solution during slab heating become incomplete, but defects may also occur on the product surface. Therefore, the total content of at least one of S and Se is preferably 0.050% or less.
[0113] (Other elements)
[0114] The above-mentioned component composition may further contain at least one element (for convenience, referred to as "element a") selected from Cu: less than 0.20%, Ni: less than 0.50%, Cr: less than 0.50%, Sb: less than 0.10%, Sn: less than 0.50%, Mo: less than 0.50% and Bi: less than 0.10%.
[0115] These elements a are easy to segregate at the grain boundaries and function as auxiliary inhibitors, thereby further improving the magnetic properties. However, if the element a is too much, secondary recrystallization is sometimes prone to occur. Therefore, the content of element a is preferably within the above range.
[0116] Furthermore, from the viewpoint of obtaining the effect of addition of the element a, the contents of Cu, Ni, Cr, Sb, Sn and Mo are each preferably 0.010% or more, and the content of Bi is preferably 0.0010% or more.
[0117] The above-mentioned component composition may further contain at least one element (for convenience, referred to as "element b") selected from B: less than 0.010%, Ge: less than 0.10%, As: less than 0.10%, P: less than 0.10%, Te: less than 0.10%, Nb: less than 0.10%, Ti: less than 0.10% and V: less than 0.10%.
[0118] The element b further enhances the grain growth inhibition and stably obtains a higher magnetic flux density. From the viewpoint of obtaining the addition effect of the element b, the contents of B and Ge are preferably 0.0010% or more, and the contents of As, P, Te, Nb, Ti and V are preferably 0.0050% or more.
[0119] (Remainder)
[0120] The remainder of the above composition is composed of Fe and inevitable impurities.
[0121] 《Manufacturing method》
[0122] Next, an example of a method for producing an electromagnetic steel sheet having a forsterite film will be described.
[0123] First, the steel having the above-mentioned component composition is melted by a conventionally known refining process, and a steel slab is obtained by a continuous casting method or an ingot-blowing method.
[0124] Next, the obtained steel slab is hot rolled to form a hot rolled sheet, and the hot rolled sheet is annealed as needed. Then, cold rolling is performed once or twice or more including intermediate annealing to obtain a cold rolled sheet of the final sheet thickness. Then, the obtained cold rolled sheet is subjected to a recrystallization annealing and a decarburization annealing, and then, an annealing separator containing MgO is applied and a final finish annealing is performed.
[0125] In this way, an electromagnetic steel sheet having a film containing forsterite (forsterite film) formed on the surface is obtained.
[0126] <Method for manufacturing electrical steel sheet with insulating coating>
[0127] Next, a method for producing an electrical steel sheet with an insulating coating will be described.
[0128] Preprocessing
[0129] First, the electromagnetic steel sheet having the forsterite film is pretreated using a pretreatment liquid. That is, the pretreatment liquid is brought into contact with the forsterite film.
[0130] The method of pretreatment is not particularly limited as long as the pretreatment solution can be brought into contact with the forsterite film. For example, a method of immersing the electromagnetic steel sheet having the forsterite film in a bath of the pretreatment solution can be cited. In this case, the following pretreatment conditions (pretreatment temperature and pretreatment time) are preferably satisfied.
[0131] (Pretreatment temperature)
[0132] In order to fully obtain the effect of the pretreatment, the pretreatment temperature (temperature of the pretreatment liquid) is preferably 30° C. or higher, more preferably 40° C. or higher.
[0133] On the other hand, if the pretreatment temperature is too high, the forsterite film may be damaged and the adhesion may be reduced. In addition, acid fume countermeasures may be required, which is not economical in this case.
[0134] Therefore, the pretreatment temperature is preferably 95°C or lower, more preferably 90°C or lower.
[0135] (Preprocessing time)
[0136] In order to fully obtain the effect of the pretreatment, the pretreatment time (the contact time between the pretreatment solution and the forsterite film) is preferably 1.0 second or longer, and more preferably 2.0 seconds or longer.
[0137] On the other hand, if the pretreatment time is too long, the pretreatment device may become redundant. In this case, it is uneconomical as in the case where acid fume countermeasures are required. In addition, if the pretreatment time is too long, the forsterite film may be damaged and the adhesion may be reduced.
[0138] Therefore, the pretreatment time is preferably 40 seconds or less, more preferably 30 seconds or less.
[0139] The forsterite film after contacting the pretreatment liquid is preferably washed with water.
[0140] It should be noted that the forsterite film does not necessarily need to be dried before applying the insulating film treatment liquid, but it is preferably dried from the viewpoint of facilitating control of the film thickness of the insulating film.
[0141] 《Coating and sintering of insulation coating treatment liquid》
[0142] Next, the insulating film treatment solution is applied to the forsterite film that has been in contact with the pretreatment solution, dried as necessary, and then sintered. Instead of sintering, planarization annealing that also serves as sintering may be performed.
[0143] In this way, an insulating film is formed on the forsterite film. That is, an electromagnetic steel sheet with an insulating film is obtained.
[0144] Example
[0145] Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited to the Examples described below.
[0146] <Manufacturing of electrical steel sheets with insulating coating>
[0147] The electrical steel sheet with an insulating coating is produced as follows.
[0148] 《Preparation of electromagnetic steel sheet with forsterite coating》
[0149] First, a grain-oriented electrical steel sheet having a thickness of 0.20 mm and having been subjected to final annealing was prepared. Due to the final annealing, a forsterite film was formed on the surface of the steel sheet.
[0150] In addition, the S amount (that is, the amount of sulfur contained in either the forsterite film or the steel sheet) of the prepared grain-oriented electrical steel sheet was determined by the method described later and the result was 50 mass ppm.
[0151] Similarly, the Se amount (that is, the amount of selenium contained in either the forsterite film or the steel sheet) of the prepared grain-oriented electrical steel sheet was determined by the method described later and found to be 100 mass ppm.
[0152] Furthermore, the forsterite film was peeled off from the prepared grain-oriented electrical steel sheet by the method described below to obtain only the steel sheet. The S and Se contents of the steel sheet in this state were determined in the same manner as above, and the results were both less than the quantitative limit.
[0153] Therefore, it is understood that in the prepared grain-oriented electrical steel sheet, most of S and Se, which are impurity elements, are mixed in the forsterite film.
[0154] 《Preparation of insulation coating treatment liquid》
[0155] Insulation film treatment solutions A to V having the component compositions shown in Table 1 below were prepared.
[0156] As the phosphate, dihydrogen phosphate was used. In addition, in the following Table 1, magnesium dihydrogen phosphate is represented as "Mg phosphate". The same applies to other dihydrogen phosphates.
[0157] As the borate, borax (Na2B4O5(OH)4·8H2O) was used.
[0158] As silicate, sodium silicate (Na3SiO3) was used.
[0159] As colloidal silica, SNOWTEX 30 manufactured by Nissan Chemical Co., Ltd. was used.
[0160] As the metal compound (compound containing a metal element), in addition to water-soluble CrO3, TiO2, ZrO2, HfO2, Nb2O5, VN, MgO or ZnO is used. The content calculated as the metal element is recorded in Table 1 below (abbreviated as "content" in Table 1 below).
[0161] The particle size of the metal compound is in the range of 0.1 to 0.8 μm. The particle size is measured using a laser diffraction particle size distribution analyzer SALD-3100 manufactured by Shimadzu Corporation. The particle size is the average particle size, which indicates the median particle size at which 50% of the particles are present on a volume basis.
[0162] 《Preparation of pretreatment solution》
[0163] Pretreatment solutions No. 1 to 51 shown in Table 2 below were prepared.
[0164] Specifically, hydrochloric acid (concentration: 35 mass %), sulfuric acid (concentration: 97 mass %), phosphoric acid (concentration: 85 mass %) and acetic acid (concentration: 99.7 mass %) as special grade liquid reagents are added to pure water in the amounts shown in Table 2 below to obtain a pretreatment solution.
[0165] The contents of the inorganic acid and acetic acid in the obtained pretreatment liquid are shown in Table 2 below.
[0166] Preprocessing
[0167] The prepared grain-oriented electrical steel sheet that has been subjected to final annealing was washed with water to remove the unreacted annealing separator, and then immersed in a bath of a pretreatment solution under the pretreatment conditions (pretreatment temperature and pretreatment time) shown in Table 2 below, and then washed with water and dried. In this way, the pretreatment was performed.
[0168] 《Coating and sintering of insulation coating treatment liquid》
[0169] After the pretreatment, the surface of the grain-oriented electrical steel sheet (i.e., the forsterite film) that has been subjected to the final annealing has a total coating weight of 12.0 g / m2 on both sides after coating and sintering. 2 Insulation coating treatment solution shown in Table 2 below was applied by a roll coater and sintered to form an insulation coating. The sintering conditions were N2: 100 volume % atmosphere, 840° C., and 20 seconds. Thus, an electromagnetic steel sheet with an insulation coating was obtained.
[0170] The magnetic flux density B8 (magnetic flux density at a magnetizing force of 800 A / m) of the obtained electromagnetic steel sheet with an insulating coating was 1.920 T.
[0171] <evaluate>
[0172] The obtained electrical steel sheets with insulating coatings were evaluated by the following methods. The evaluation results are shown in Table 2 below.
[0173] S-Quantity
[0174] (Before peeling)
[0175] The S content (unit: mass ppm) of the obtained electrical steel sheet with an insulating coating was determined in accordance with the combustion-infrared absorption method described in JIS G 1215-4.
[0176] The obtained S amount refers to the amount of sulfur (S) contained in any one of the insulating film, the forsterite film, and the steel sheet.
[0177] (After peeling)
[0178] The obtained electrical steel sheet with insulation coating was immersed in a mixed solution of hydrochloric acid and hydrofluoric acid to remove the insulation coating and forsterite coating to form a steel sheet alone. The S content (unit: mass ppm) of the steel sheet in this state was determined in the same manner as above.
[0179] "Color"
[0180] (Before peeling)
[0181] The Se amount (unit: mass ppm) of the obtained electrical steel sheet with an insulating coating was determined.
[0182] The amount of Se can be determined based on its size by the atomic absorption spectrophotometry described in JIS G 1257-20 or the 2,3-diaminonaphthalene extraction absorptiometry described in JIS G 1233.
[0183] The Se amount obtained is the amount of selenium (Se) contained in any one of the insulating film, the forsterite film, and the steel sheet.
[0184] (After peeling)
[0185] The obtained electrical steel sheet with insulation coating was immersed in a mixed solution of hydrochloric acid and hydrofluoric acid to remove the insulation coating and forsterite coating to form a steel sheet alone. The Se content (unit: mass ppm) of the steel sheet in this state was determined in the same manner as above.
[0186] In addition, when the amount of S and the amount of Se were less than the quantitative limit, "ND" was written in the corresponding column of the following Table 2.
[0187] 《Fitness》
[0188] The obtained electrical steel sheet with an insulating coating was subjected to stress relief annealing at 820° C. for 3 hours in a nitrogen atmosphere.
[0189] The electromagnetic steel sheet with insulation coating after stress relief annealing was wound on round bars with different diameters at intervals of 5 mm, such as 5 mm, 10 mm, etc., to find the minimum diameter at which the forsterite coating did not peel off. When the diameter was 30 mm or less, it was evaluated that the forsterite coating had excellent adhesion to the steel sheet.
[0190] Iron Loss
[0191] A test piece of 30 mm in width and 280 mm in length was cut out from the obtained electromagnetic steel sheet with an insulating coating. The iron loss (W) was measured using the cut test piece according to the method described in JIS C 2550. 17 / 50 ) (Magnetic flux density amplitude 1.7T, frequency 50Hz unit mass loss). Iron loss (W 17 / 50 ) is preferably less than 0.800 W / kg.
[0192] [Table 1]
[0193]
[0194]
[0195]
[0196]
[0197] 〈Summary of evaluation results〉
[0198] As shown in Table 2, the electrical steel sheets with insulating coatings of Nos. 4 to 9, 12 to 16, 19 to 39, and 41 to 51 (invention examples) have excellent adhesion of the forsterite coating and low iron loss.
[0199] On the other hand, the electrical steel sheets with insulating coatings of Nos. 1 to 3, 10 to 11, 17 to 18, and 40 (Comparative Examples) were insufficient in at least one of the adhesion of the forsterite coating and the reduction of the iron loss.
[0200] 《Comparison of No.1 to 10》
[0201] Here, among Nos. 1 to 51, Nos. 1 to 10 using the insulating film treatment liquid A are representatively compared.
[0202] First, reference is made to No. 1 using a pretreatment liquid not containing acetic acid.
[0203] Since No. 1 has a large amount of S (before stripping) and Se (before stripping), it can be seen that the impurity elements (S and Se) in the forsterite film are sufficiently removed by the pretreatment using the pretreatment liquid.
[0204] In addition, since No. 1 also has large amounts of S (after stripping) and Se (after stripping), it is known that impurity elements (S and Se) re-enter the steel sheet from the forsterite film during sintering for forming the insulating film.
[0205] No. 2 is an example in which a pretreatment liquid not containing acetic acid is used in the same manner as No. 1, but the pretreatment time is made longer than that of No. 1.
[0206] In No. 2, the amount of S and Se are reduced compared to No. 1, and it is understood that S and Se in the forsterite film are removed by prolonging the pretreatment time.
[0207] However, the adhesion and iron loss reduction of No. 2 were not sufficient. This is presumably because the forsterite film was damaged due to the prolonged pretreatment time.
[0208] No. 3 is an example in which a pretreatment liquid not containing acetic acid is used similarly to No. 1, but the pretreatment temperature is higher than that of No. 1.
[0209] In No. 3, the amount of S and Se are reduced compared to No. 1, and it is understood that S and Se in the forsterite film are removed by increasing the pretreatment temperature.
[0210] However, the adhesion and iron loss reduction of No. 3 were not sufficient. This is presumably because the forsterite film was damaged due to the increase in the pretreatment temperature.
[0211] On the other hand, reference is made to Nos. 4 to 10 using a pretreatment liquid containing acetic acid.
[0212] In No. 4 to 9, even under the same pretreatment conditions (pretreatment temperature and pretreatment time) as No. 1, the S amount and Se amount were reduced compared with No. 1, and it was found that S and Se in the forsterite film were removed.
[0213] In addition, in Nos. 4 to 9, the adhesion of the forsterite film was good and the iron loss was low, and the damage of the forsterite film due to the pretreatment was suppressed.
[0214] However, in No. 10 using a pretreatment liquid containing a large amount of acetic acid, the amount of S and Se was not sufficiently reduced. This is presumably because, as described above, the amount of S and Se adsorbed by acetic acid increased, causing steric hindrance and reducing the dissolution rate.
[0215] In such No. 10, the forsterite film was not damaged and the adhesion was good, but S and Se again penetrated into the steel sheet from the forsterite film, and the reduction of the iron loss was insufficient.
Claims
1. A pretreatment solution used before applying an insulating coating treatment solution containing at least one salt selected from phosphates, borates and silicates to an electromagnetic steel sheet having a forsterite coating on its surface, The pretreatment solution contains at least one inorganic acid selected from hydrochloric acid, sulfuric acid and phosphoric acid and acetic acid, The content of the acetic acid is 1 to 3000 ppm by mass.
2. The pretreatment solution according to claim 1, wherein The content of the inorganic acid is 0.20 mass % to 30.00 mass %.
3. A method for manufacturing an electromagnetic steel sheet with an insulating coating, comprising pretreating an electromagnetic steel sheet having a forsterite coating on its surface using the pretreatment solution according to claim 1 or 2, and then applying an insulating coating treatment solution containing at least one salt selected from phosphates, borates and silicates and then sintering to form an insulating coating.
4. The method for producing an electrical steel sheet with an insulating coating according to claim 3, wherein: The pretreatment is a treatment in which the pretreatment liquid is brought into contact with the forsterite film.
5. The method for producing an electrical steel sheet with an insulating coating according to claim 4, wherein: The temperature of the pretreatment liquid is 30°C to 95°C The contact time between the pretreatment liquid and the forsterite film is 1.0 second to 40 seconds.
6. The method for producing an electrical steel sheet with an insulating coating according to any one of claims 3 to 5, wherein: The content of the chromium compound in the insulating film treatment liquid is 1.0 part by mass or less in terms of chromium element relative to 100 parts by mass of the salt.