Aerogel atomizing core and preparation method thereof, atomizer and electronic atomizing device
By preparing through holes or blind holes in the atomizing core and filling them with SiC nanowires or Si3N4 nanowires, the contradiction between the pore size and strength of the atomizing core is resolved, the service life is improved and the production cost is reduced, while maintaining the atomization effect.
Patent Information
- Application Number
- CN202411152108.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
The pore size of existing atomizer cores affects the atomization effect and e-liquid supply speed. Furthermore, the larger the pore size of an aerogel atomizer core, the lower its strength, resulting in a shorter lifespan.
Laser processing is used to prepare through holes or blind holes on porous ceramic materials, and SiC nanowires or Si3N4 nanowires are grown in situ in the holes as filling components to increase the pore size and maintain strength. An oleophobic layer is set on the ceramic aerogel component to prevent clogging.
It achieves a balance between aperture size and strength, improves the lifespan of the atomizer core and reduces production costs, while avoiding oil leakage and maintaining the atomization effect.
Smart Images

Figure CN118902181A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electronic cigarettes, and in particular to an aerogel atomization core and a preparation method thereof, an atomizer and an electronic atomization device. Background Art
[0002] The core component of electronic cigarettes is the atomizer core, which mainly heats and atomizes the e-liquid to produce smoke for users to inhale. At present, the main material of the atomizer core is porous ceramics, and the size of the porous ceramic aperture directly affects the atomization effect and the supply speed of the e-liquid. However, the larger the aperture of the aerogel atomizer core, the lower the strength of the aerogel atomizer core, which brings challenges to the design and manufacture of the atomizer core. In traditional technology, although there is a solution of using laser drilling on the aerogel atomizer core, it cannot improve the strength of the aerogel atomizer core; in addition, there are also silicon wafers or glass parts that are engraved with multiple micropores or pores arranged according to preset rules by laser and other processing methods for oil conduction, and the processing cost of micropores or pores is relatively high. Summary of the invention
[0003] Based on this, it is necessary to provide an aerogel atomizer core. The aerogel atomizer core of the present invention can achieve a balance between the atomizer core pore size and the atomizer core strength, thereby increasing the service life of the atomizer core.
[0004] An embodiment of the present application provides an aerogel atomization core.
[0005] An aerogel atomization core comprises a ceramic aerogel component, a filling component and a heating component, wherein the ceramic aerogel component comprises a first surface and a second surface arranged at relative positions, the ceramic aerogel component is provided with a first guide hole extending from the first surface to the second surface, the filling component is filled in the first guide hole, the porosity of the filling component is greater than the porosity of the ceramic aerogel component and / or the pore size of the filling component is greater than the pore size of the ceramic aerogel component, and the heating component is connected to the second surface.
[0006] In some embodiments, the first guide hole is a blind hole, the blind hole opens on the first surface, and the depth of the blind hole extending from the first surface to the second surface is 1 mm to 3 mm.
[0007] In some embodiments, the first guide hole is a through hole, one end of the first guide hole opens to the first surface and the other end of the first guide hole opens to the second surface.
[0008] In some embodiments, there are multiple first guide holes, the multiple first guide holes are spaced apart, and each first guide hole is filled with the filling component.
[0009] And / or, the first guide hole is a cylindrical hole, and the hole diameter of the first guide hole is 0.1mm~1mm.
[0010] In some embodiments, the filling component includes but is not limited to SiC nanowires and / or Si3N4 nanowires.
[0011] In some of the embodiments, a second guide hole is further provided on the ceramic aerogel component, and the aperture of the second guide hole is 0.001 mm to 0.15 mm.
[0012] In some embodiments, the preparation material of the ceramic aerogel component includes one or more of a carbon source, a nitrogen source and a silicon source.
[0013] In some of the embodiments, the ceramic aerogel component is prepared by using a dry pressing process, a tape casting process, a hot die casting process or a slip injection process, and then a sintering process.
[0014] In some embodiments, the porosity of the ceramic aerogel component is 50% to 70%;
[0015] And / or, the pore size of the ceramic aerogel component is 0.5 μm-60 μm.
[0016] In some embodiments, the porosity of the filling component is 60%-90%;
[0017] And / or, the pore size of the filling component is 1 μm to 80 μm.
[0018] In some embodiments, the heating component includes one or more of a resistance wire, an etched mesh, and a thick film printed circuit.
[0019] In some embodiments, the aerogel atomization core further includes an oleophobic layer, which covers and is connected to the first surface, and is used to prevent the aerosol-generating matrix from adhering to and blocking the first guide hole.
[0020] In some of the embodiments, an oil storage tank is provided on the first surface of the ceramic aerogel component, and the depth of the oil storage tank is 1 mm to 1.6 mm. When the first guide hole is a through hole, the two ends of the first guide hole are respectively opened to the bottom surface of the oil storage tank and the second surface. When the first guide hole is a blind hole, the first guide hole is opened to the bottom surface of the oil storage tank.
[0021] An embodiment of the present application also provides a method for preparing the aerogel atomization core.
[0022] A method for preparing the aerogel atomization core comprises the following steps:
[0023] Preparing a first guide hole on the ceramic aerogel component, wherein the first guide hole extends from the first surface to the second surface of the ceramic aerogel component;
[0024] preparing a filling component in the first guide hole, wherein the porosity of the filling component is greater than the porosity of the ceramic aerogel component and / or the pore size of the filling component is greater than the pore size of the ceramic aerogel component; and
[0025] A heating component is connected to the second surface of the ceramic aerogel component to obtain an aerogel atomization core.
[0026] In some embodiments, the preparation of the first guide hole on the ceramic aerogel component includes the following steps:
[0027] The green body required for preparing the ceramic aerogel component is placed in a laser and mechanical processing device, and a through hole and / or a blind hole with a diameter of 0.1 mm to 1 mm is prepared on the green body as a first guide hole.
[0028] In some embodiments, preparing the filling component in the first guide hole includes the following steps:
[0029] The green body with the first guide hole is placed in a sintering furnace for in-situ growth of SiC nanowires and / or Si3N4 nanowires, the temperature is set to 1000℃~1800℃, the time is 1h~8h, the pressure is 0.01MPa~1MPa, argon or nitrogen is introduced, and the diameters of the SiC nanowires and / or Si3N4 nanowires are 5nm~200nm respectively.
[0030] In some of the embodiments, the method for preparing the aerogel atomization core further comprises the following step: subjecting the prepared aerogel atomization core to high temperature treatment.
[0031] An embodiment of the present application also provides an atomizer.
[0032] An atomizer comprises the aerogel atomization core, or the aerogel atomization core prepared by the preparation method.
[0033] An embodiment of the present application also provides an electronic atomization device.
[0034] An electronic atomization device comprises the atomizer and a power supply component, wherein the power supply component is electrically connected to a heating component of the aerogel atomization core in the atomizer.
[0035] Compared with the prior art, the present application can increase the aperture of the first guide hole while maintaining the strength of the ceramic aerogel component, achieving a balance between the two and having obvious cost and quality advantages.
[0036] The above-mentioned aerogel atomization core can be processed by laser to prepare through holes or blind holes on the existing porous ceramic material, and then filler components can be prepared in the through holes or blind holes, such as in-situ growth of SiC nanowires and / or Si3N4 nanowires, so as to increase the filling components without reducing the strength of the porous ceramic material too much, and set the porosity and pore size of the filling components to be larger than the ceramic aerogel components, thereby increasing the overall average pore size of the aerogel atomization core, thereby solving the contradiction between the pore size of the aerogel atomization core for electronic cigarettes and the strength of the aerogel atomization core in the traditional technology, and increasing the service life of the aerogel atomization core. Furthermore, the SiC nanowires and / or Si3N4 nanowires grown in the present application will not cause the electronic cigarette cartridge to leak oil, thereby reducing the production cost and avoiding the possible impact on the atomization effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0038] In order to more completely understand the present application and its beneficial effects, the following description will be given in conjunction with the accompanying drawings. In the following description, the same reference numerals represent the same parts.
[0039] Figure 1 This is a schematic diagram of the aerogel atomization core described in Example 1 of the present invention;
[0040] Figure 2 This is a schematic diagram of the aerogel atomization core described in Example 1 of the present invention from another angle;
[0041] Figure 3 This is a cross-sectional schematic diagram of the aerogel atomization core described in Example 1 of the present invention;
[0042] Figure 4 This is a cross-sectional schematic diagram of the aerogel atomization core described in Example 3 of the present invention;
[0043] Figure 5 This is a cross-sectional schematic diagram of the aerogel atomization core described in Example 4 of the present invention;
[0044] Figure 6 This is a cross-sectional schematic diagram of the aerogel atomization core described in Example 5 of the present invention;
[0045] Figure 7 This is a front schematic diagram of the aerogel atomization core described in Example 6 of the present invention;
[0046] Figure 8This is a front schematic diagram of the aerogel atomization core described in Example 7 of the present invention;
[0047] Fig. 9 This is a cross-sectional schematic diagram of the aerogel atomization core described in Example 7 of the present invention;
[0048] Fig.10 This is a schematic cross-sectional view of the aerogel atomization core described in Example 8 of the present invention.
[0049] Description of Reference Numerals
[0050] 10. Aerogel atomization core; 100. Ceramic aerogel component; 101. First surface; 102. Second surface; 103. First guide hole; 104. Oil storage tank; 200. Filling component; 300. Heating component; 400. Oleophobic layer. DETAILED DESCRIPTION
[0051] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0052] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0053] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0054] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0055] In the description of the present invention, "several" means more than one, "many" means more than two, "greater than", "less than", "exceed" etc. are understood to exclude the number itself, and "above", "below", "within" etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing the technical features, and cannot be understood as indicating or implying the relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0056] In this article, unless otherwise stated, each reaction step may be carried out in the order described herein or may not be carried out in the order described herein. For example, other steps may be included between each reaction step, and the order of the reaction steps may also be appropriately swapped. This can be determined by the technician based on common knowledge and experience. Preferably, the reaction method herein is carried out sequentially.
[0057] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for a broad range of quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.
[0058] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0059] The embodiment of the present application provides an aerogel atomizer core 10 to solve the problem that the size of the porous ceramic pore size of the existing atomizer core affects the atomization effect and the supply speed of the e-liquid, and the larger the pore size of the aerogel atomizer core 10, the lower the strength of the aerogel atomizer core 10. The aerogel atomizer core 10 will be described below in conjunction with the accompanying drawings.
[0060] The aerogel atomization core 10 provided in the embodiment of the present application is exemplary, see Figure 1 As shown, Figure 1 The aerogel atomization core 10 provided in the embodiment of the present application is a schematic diagram of the structure of the aerogel atomization core 10. The aerogel atomization core 10 of the present application can be used for electronic cigarettes.
[0061] In order to more clearly illustrate the structure of the aerogel atomization core 10 , the aerogel atomization core 10 will be introduced below with reference to the accompanying drawings.
[0062] For example, see Figure 1 As shown, an aerogel atomization core 10 includes a ceramic aerogel component 100, a filling component 200 and a heating component 300. The ceramic aerogel component 100 includes a first surface 101 and a second surface 102 arranged at relative positions. The ceramic aerogel component 100 is provided with a first guide hole 103 extending from the first surface 101 to the second surface 102. The filling component 200 is filled in the first guide hole 103. The porosity of the filling component 200 is greater than the porosity of the ceramic aerogel component 100 and / or the pore size of the filling component 200 is greater than the pore size of the ceramic aerogel component 100. The heating component 300 is connected to the second surface 102.
[0063] In some embodiments, the first guide hole 103 is a blind hole. The blind hole opens on the first surface 101, and the depth of the blind hole extending from the first surface 101 to the second surface 102 is 1 mm to 3 mm. The depth of the blind hole extending from the first surface 101 to the second surface 102 includes but is not limited to: 1 mm, 2 mm, 3 mm, or a range between any two of the foregoing.
[0064] In some embodiments, the first guide hole 103 is a through hole. One end of the first guide hole 103 opens on the first surface 101 and the other end opens on the second surface 102 .
[0065] In some embodiments, there are multiple first guide holes 103. The multiple first guide holes 103 are distributed at intervals, and each first guide hole 103 is filled with a filling component 200.
[0066] In some embodiments, the number of the first guide holes 103 is 1 to 10, preferably 3 to 5.
[0067] In some embodiments, the first guide hole 103 is a cylindrical hole, and the diameter of the first guide hole 103 is 0.1 mm to 1 mm. The diameter of the first guide hole 103 includes but is not limited to: 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm or a range between any two of the foregoing.
[0068] In some of the embodiments, the filler feature 200 includes SiC nanowires and / or Si 3 N 4 nanowires.
[0069] In some embodiments, the preparation material of the ceramic aerogel component 100 includes one or more of a carbon source, a nitrogen source, and a silicon source. For example, the preparation material of the ceramic aerogel component 100 includes diatomaceous earth, quartz sand, and ceramic fiber. Among them, the ceramic fiber includes one or more of alumina ceramics, silicon carbide ceramics, silicon nitride ceramics, aluminum nitride ceramics, silicon oxide ceramics, and cordierite ceramics.
[0070] In some of the embodiments, the ceramic aerogel component 100 is prepared by using a dry pressing process, a tape casting process, a hot pressing process or a slip injection process.
[0071] In some of the embodiments, a second guide hole is also provided on the ceramic aerogel component 100, and the aperture of the second guide hole is 0.001mm~0.15mm. The second guide hole is not shown in the drawings. The aperture value of the second guide hole includes but is not limited to: 0.001mm, 0.05mm, 0.01mm, 0.03mm, 0.05mm, 0.08mm, 0.1mm, 0.12mm, 0.15mm or a range between any two of the foregoing. The second guide hole is not filled with a filling component 200, and the function of the second guide hole is to increase the porosity of the ceramic aerogel component 100. It should be noted that the extension direction of the second guide hole in the present application is not necessarily a straight line, but may also be curved or circuitous. The second guide hole is formed during the sintering process of the green body, and the second guide hole makes the ceramic aerogel component 100 have a porous structure. Furthermore, when the SiC nanowires and / or Si3N4 nanowires are grown in situ, some of the SiC nanowires and / or Si3N4 nanowires will extend into the second guide holes.
[0072] In some embodiments, the porosity of the ceramic aerogel component 100 is 50% to 70%. Preferably, 45% to 65%. For example, the porosity of the ceramic aerogel component 100 includes but is not limited to: 50%, 55%, 60%, 65%, 70% or a range between any two of the foregoing.
[0073] In some embodiments, the pore size of the ceramic aerogel component 100 is 0.5 μm to 60 μm. The pore size of the ceramic aerogel component 100 includes, but is not limited to, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, or a range between any two of the foregoing.
[0074] In some embodiments, the porosity of the filling component 200 is 60%-90%. For example, the porosity of the filling component 200 includes but is not limited to: 60%, 65%, 70%, 80%, 85%, 90% or a range between any two of the foregoing.
[0075] In some embodiments, the pore size of the filling component is 1 μm to 80 μm. The pore size of the filling component 200 includes but is not limited to: 1 μm, 1.5 μm, 5 μm, 10 μm, 15 μm, 30 μm, 35 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm or a range between any two of the foregoing.
[0076] In some embodiments, the heating component 300 includes one or more of a resistance wire, an etched mesh, and a thick film printed circuit. Preferably, the heating component 300 is in the form of a thick film printed circuit.
[0077] In some embodiments, the aerogel atomization core 10 further includes an oleophobic layer 400. The oleophobic layer 400 covers and is connected to the first surface 101. The oleophobic layer 400 is used to prevent the aerosol-generating matrix from adhering to the surface of the aerogel atomization core 10 and blocking the first guide hole 103 or the second guide hole.
[0078] In some of the embodiments, the first surface 101 of the ceramic aerogel component 100 is provided with an oil storage groove 104. The depth of the oil storage groove 104 is 1 mm to 1.6 mm. The depth of the oil storage groove 104 includes but is not limited to: 1 mm, 1.2 mm, 1.4 mm, 1.5 mm, 1.6 mm or a range between any two of the foregoing. When the first guide hole 103 is a through hole, the two ends of the first guide hole 103 are respectively opened at the bottom surface of the groove of the oil storage groove 104 and the second surface 102, and similarly, the two ends of the second guide hole are respectively opened at the bottom surface of the groove of the oil storage groove 104 and the second surface 102. When the first guide hole 103 is a blind hole, the first guide hole 103 is opened at the bottom surface of the groove of the oil storage groove 104, and similarly, the second guide hole is opened at the bottom surface of the groove of the oil storage groove 104.
[0079] An embodiment of the present application also provides a method for preparing an aerogel atomization core 10 .
[0080] A method for preparing an aerogel atomization core 10 comprises the following steps:
[0081] S1. Prepare a first guide hole 103 on the ceramic aerogel component 100 , wherein the first guide hole 103 extends from the first surface 101 to the second surface 102 of the ceramic aerogel component 100 .
[0082] S2, preparing a filling component 200 in the first guide hole 103, wherein the porosity of the filling component 200 is greater than the porosity of the ceramic aerogel component 100 and / or the pore size of the filling component 200 is greater than the pore size of the ceramic aerogel component 100.
[0083] S3, connecting the heating component 300 to the second surface 102 of the ceramic aerogel component 100 to obtain the aerogel atomization core 10.
[0084] In some embodiments, the preparation of the first guide hole 103 on the ceramic aerogel component 100 includes the following steps:
[0085] The green body required for preparing the ceramic aerogel component 100 is placed in a laser and mechanical processing device, and the laser power is set to 50W~100W, the frequency is 10kHz~20kHz, and the speed is 100mm / s~200mm / s. Through holes and / or blind holes with a diameter of 0.1mm~1mm are prepared on the green body as the first guide holes 103.
[0086] In some embodiments, when preparing the filling component 200 in the first guide hole 103, the following steps are included:
[0087] The green body with the first guide hole 103 is placed in a sintering furnace to in-situ grow SiC nanowires and / or Si3N4 nanowires, the temperature is set to 1000°C to 1800°C, the time is 1h to 8h, the pressure is 0.01MPa to 1MPa, argon or air is introduced, and the diameters of the SiC nanowires and / or Si3N4 nanowires are 5nm to 200nm respectively. When sintering in the sintering furnace, the green body can be sintered into a ceramic aerogel component 100.
[0088] In some embodiments, the method for preparing the aerogel atomization core 10 further includes the following steps:
[0089] S4, subjecting the prepared aerogel atomization core 10 to high temperature treatment.
[0090] In some of the embodiments, when the prepared aerogel atomization core 10 is subjected to high temperature treatment in step S4, the following steps are included: placing the aerogel atomization core 10 in a high temperature furnace, setting the temperature to 800°C~1500°C, the time to 1h~4h, the pressure to 1atm~1.5atm, and the argon flow rate to 5sccm~10sccm.
[0091] An embodiment of the present application also provides an atomizer.
[0092] An atomizer includes the above-mentioned aerogel atomization core 10, or the aerogel atomization core 10 prepared by the above-mentioned preparation method.
[0093] An embodiment of the present application also provides an electronic atomization device.
[0094] An electronic atomization device comprises the atomizer and a power supply assembly, wherein the power supply assembly is electrically connected to a heating component 300 of an aerogel atomization core 10 in the atomizer.
[0095] For example, the electronic atomization device described above can be applied to the field of electronic cigarettes to prepare electronic cigarettes.
[0096] Furthermore, an embodiment of the present application provides an electronic cigarette.
[0097] An electronic cigarette comprises the above-mentioned aerogel atomization core 10, or the aerogel atomization core 10 prepared by the above-mentioned preparation method.
[0098] Example 1
[0099] This embodiment provides an aerogel atomization core 10 .
[0100] See also Figure 1-Figure 3As shown, the aerogel atomization core 10 of the present embodiment includes a ceramic aerogel component 100, a filling component 200 and a heating component 300. The length, width and thickness of the ceramic aerogel component 100 are 6mm*3mm*3mm, respectively. The porosity of the ceramic aerogel component 100 is 30%, and the pore size of the ceramic aerogel component 100 is 0.5μm. The preparation materials of the ceramic aerogel component 100 include diatomaceous earth, quartz sand and alumina powder. The preparation materials of the ceramic aerogel component 100 are first prepared into a green body, and the green body is prepared by a grouting molding process. The ceramic aerogel component 100 includes a first surface 101 and a second surface 102 arranged in relative positions. Three first guide holes 103 extending from the first surface 101 to the second surface 102 are provided on the ceramic aerogel component 100. The first guide holes 103 are distributed at intervals, and the first guide holes 103 are through holes. One end of the first guide hole 103 opens at the first surface 101 and the other end opens at the second surface 102 . The first guide hole 103 is a cylindrical hole, and the hole diameter of the first guide hole 103 is 0.1 mm.
[0101] Each first guide hole 103 is filled with SiC nanowires as a filling member 200 . The porosity of the filling member 200 is 60%, and the pore size of the filling member 200 is 1 μm. The heating member 300 is connected to the second surface 102 .
[0102] The aerogel atomization core 10 of this embodiment is prepared by the following preparation method. The preparation method of the aerogel atomization core 10 comprises the following steps:
[0103] S1. Use diatomite, quartz sand and alumina powder to prepare a green body by slip casting process, wherein the shape of the green body is substantially the same as the shape of the ceramic aerogel component 100 to be prepared. Put the green body into laser and mechanical processing equipment, set the laser power to 100W, the frequency to 20kHz, and the speed to 100mm / s, and prepare a through hole with a diameter of 0.1mm on the green body as the first guide hole 103. The first guide hole 103 extends from the first surface 101 to the second surface 102 of the green body.
[0104] S2, placing the green ceramic material with the first guide hole 103 into a sintering furnace to in-situ grow SiC nanowires, setting the temperature to 1500°C, the time to 3 hours, the pressure to 1 MPa, and passing argon. The prepared SiC nanowires have a porosity of 35%, a diameter of 50 nm, and a pore size of 0.8 μm, and a ceramic aerogel component 100 is obtained, wherein a plurality of second guide holes are formed on the ceramic aerogel component 100 after sintering, so that the ceramic aerogel component 100 has a porous structure.
[0105] S3, connecting the heating component 300 to the second surface 102 of the ceramic aerogel component 100 to obtain the aerogel atomization core 10.
[0106] S4, subjecting the prepared aerogel atomization core 10 to high temperature treatment, placing the aerogel atomization core 10 in a high temperature furnace, setting the temperature to 800° C., the time to 4 h, the pressure to 1 atm, and the argon flow rate to 10 sccm.
[0107] Example 2
[0108] This embodiment provides an aerogel atomization core 10 .
[0109] See also Figure 1-Figure 3 As shown, the aerogel atomization core 10 of this embodiment includes a ceramic aerogel component 100, a filling component 200 and a heating component 300. The length, width and thickness of the ceramic aerogel component 100 are 6mm*3mm*3mm, respectively. The porosity of the ceramic aerogel component 100 is 50%, and the pore size of the ceramic aerogel component 100 is 1.5μm. The material for preparing the ceramic aerogel component 100 is first prepared into a green body, and the green body is prepared by a tape casting process. The ceramic aerogel component 100 includes a first surface 101 and a second surface 102 arranged in relative positions. Three first guide holes 103 extending from the first surface 101 to the second surface 102 are provided on the ceramic aerogel component 100. The first guide holes 103 are spaced apart, and the first guide holes 103 are through holes. One end of the first guide hole 103 opens at the first surface 101 and the other end opens at the second surface 102. The first guide hole 103 is a cylindrical hole, and the aperture of the first guide hole 103 is 0.5mm.
[0110] Each first guide hole 103 is filled with SiC nanowires as a filling member 200 . The porosity of the filling member 200 is 90%, and the pore size of the filling member 200 is 80 μm. The heating member 300 is connected to the second surface 102 .
[0111] The aerogel atomization core 10 of this embodiment is prepared by the following preparation method. The preparation method of the aerogel atomization core 10 comprises the following steps:
[0112] S1. Use diatomite, quartz sand and alumina powder to prepare a green body by tape casting process, wherein the shape of the green body is substantially the same as the shape of the ceramic aerogel component 100 to be prepared. Put the green body into laser and mechanical processing equipment, set the laser power to 50W, the frequency to 20kHz, and the speed to 200mm / s, and prepare a through hole with a diameter of 0.5mm on the green body as the first guide hole 103. The first guide hole 103 extends from the first surface 101 to the second surface 102 of the green body.
[0113] S2, placing the green body with the first guide hole 103 into a sintering furnace to in-situ grow SiC nanowires, setting the temperature to 1600°C, the time to 2 hours, the pressure to 1 atm, and passing argon. The prepared SiC nanowires have a porosity of 60%, a diameter of 50 nm, and a pore size of 2 μm, and a ceramic aerogel component 100 is obtained, wherein a plurality of second guide holes are formed on the ceramic aerogel component 100 after sintering, so that the ceramic aerogel component 100 has a porous structure.
[0114] S3, connecting the heating component 300 to the second surface 102 of the ceramic aerogel component 100 to obtain the aerogel atomization core 10.
[0115] S4, subjecting the prepared aerogel atomization core 10 to high temperature treatment, placing the aerogel atomization core 10 in a high temperature furnace, setting the temperature to 1500° C., the time to 4 h, the pressure to 1.5 atm, and the argon flow rate to 10 sccm.
[0116] Example 3
[0117] This embodiment provides an aerogel atomization core 10 .
[0118] See also Figure 4 As shown, the aerogel atomization core 10 of this embodiment is basically the same as that of Embodiment 1, except that the first guide hole 103 of this embodiment is a blind hole, which opens on the first surface 101, and the depth of the blind hole extending from the first surface 101 to the second surface 102 is 1.5 mm.
[0119] Example 4
[0120] This embodiment provides an aerogel atomization core 10 .
[0121] See also Figure 5 As shown, the aerogel atomization core 10 of this embodiment is basically the same as that of Embodiment 1, except that the first guide hole 103 of this embodiment includes a through hole and a blind hole, the blind hole opens on the first surface 101, and the depth of the blind hole extending from the first surface 101 to the second surface 102 is 1.5 mm. One end of the through hole opens on the first surface 101 and the other end opens on the second surface 102, and the aperture of the first guide hole 103 of the through hole is 0.1 mm.
[0122] Example 5
[0123] This embodiment provides an aerogel atomization core 10 .
[0124] See also Figure 6As shown, the aerogel atomization core 10 of this embodiment is basically the same as that of embodiment 1, except that the first surface 101 of the ceramic aerogel component 100 in this embodiment is covered and connected with an oleophobic layer 400. The thickness of the oleophobic layer 400 is 0.1 mm. The oleophobic layer 400 is used to prevent the aerosol-generating matrix from adhering and blocking the first guide hole 103.
[0125] Example 6
[0126] This embodiment provides an aerogel atomization core 10 .
[0127] See also Figure 7 As shown, the aerogel atomization core 10 of this embodiment is substantially the same as that of the embodiment 1, except that the aerogel atomization core 10 of this embodiment includes 6 first guide holes 103 distributed in 2 rows and 3 columns.
[0128] Example 7
[0129] This embodiment provides an aerogel atomization core 10 .
[0130] See also Figure 8 , 9 As shown, the aerogel atomization core 10 of this embodiment is basically the same as that of embodiment 1, except that the first surface 101 of the ceramic aerogel component 100 in this embodiment is provided with an oil storage tank 104. The depth of the oil storage tank 104 is 1.6 mm. The first guide hole 103 is a through hole, and the two ends of the first guide hole 103 are respectively opened at the bottom surface of the oil storage tank 104 and the second surface 102.
[0131] The aerogel atomization core 10 of this embodiment is prepared by the following preparation method. The preparation method of the aerogel atomization core 10 comprises the following steps:
[0132] S1. A green body is prepared by using diatomite, quartz sand and alumina powder through a slip casting process, wherein the shape of the green body is substantially the same as the shape of the ceramic aerogel component 100 to be prepared. An oil storage groove 104 with a depth of 1.6 mm is formed on the first surface 101 of the green body by cutting, and the length of the oil storage groove 104 is 4 mm and the width is 1.6 mm.
[0133] S2, placing the blank of step S1 into a laser and mechanical processing device, setting the laser power to 100 W, the frequency to 20 kHz, and the speed to 100 mm / s, and preparing a through hole with a diameter of 0.1 mm on the blank as the first guide hole 103. The first guide hole 103 extends from the first surface 101 to the second surface 102 of the blank.
[0134] S3, placing the ceramic aerogel component 100 ceramic material with the first guide hole 103 into a sintering furnace to in-situ grow SiC nanowires, setting the temperature to 1500°C, the time to 3h, the pressure to 1.5atm, the reaction gas to silane and methane, the silane flow rate to 10sccm, and the methane flow rate to 5sccm. The prepared SiC nanowires have a porosity of 35%, a diameter of 50nm, and a pore size of 0.8μm, and a ceramic aerogel component 100 is obtained, wherein a plurality of second guide holes are formed on the ceramic aerogel component 100 after sintering, so that the ceramic aerogel component 100 has a porous structure.
[0135] S4. Connect the heating component 300 to the second surface 102 of the ceramic aerogel component 100 to obtain the aerogel atomization core 10.
[0136] S5. The prepared aerogel atomization core 10 is subjected to high temperature treatment, and the aerogel atomization core 10 is placed in a plasma device, and the temperature is set to 800° C., the time is 2 h, the pressure is 1 atm, the reaction gases are oxygen and argon, the oxygen flow rate is 20 sccm, and the argon flow rate is 10 sccm.
[0137] Example 8
[0138] This embodiment provides an aerogel atomization core 10 .
[0139] See also Fig.10 As shown, the aerogel atomization core 10 of this embodiment is basically the same as that of embodiment 7, except that the first surface 101 of the ceramic aerogel component 100 in this embodiment is provided with an oil storage tank 104. The depth of the oil storage tank 104 is 1.6 mm. The first guide hole 103 is a blind hole, which opens at the bottom surface of the oil storage tank 104, and the depth of the blind hole is 1 mm.
[0140] Comparative Example 1
[0141] This comparative example provides an aerogel atomization core.
[0142] The aerogel atomization core of this comparative example is substantially the same as that of Example 1, except that the ceramic aerogel component of the aerogel atomization core of this comparative example is not provided with air guide holes. Correspondingly, steps S1 and S2 are omitted in the preparation method.
[0143] Comparative Example 2
[0144] This comparative example provides an aerogel atomization core.
[0145] The aerogel atomization core of this comparative example is substantially the same as that of Example 1, except that no filling component is provided in the air guide hole of the ceramic aerogel component in this comparative example. Correspondingly, step S2 is omitted in the preparation method.
[0146] The performance tests were performed on the aerogel atomization cores 10 of Examples 1 to 8 and the aerogel atomization cores of Comparative Examples 1 and 2. The test results are shown in Table 1.
[0147] During the test, the porosity of the aerogel atomizer cores 10 of Examples 1 to 8 and the aerogel atomizer cores obtained in Comparative Examples 1 and 2 was measured according to the Archimedean drainage method, with reference to the national standard JIS R1634-1998.
[0148] Reference standard for strength test: The strength of each aerogel atomization core 10 is tested using the national standard "GB / T 1041-2008" method.
[0149] Oil conduction performance test method: Use cigarette oil for internal standard test, place the aerogel atomization core 10 on the test cigarette oil by titration, and observe the time for the test cigarette oil to be guided from the first surface 101 of the aerogel atomization core 10 to the second surface 102. The test cigarette oil is composed of 50% propylene glycol and 50% glycerol (propylene glycol) by mass. Each embodiment and comparative example is tested at least 3 times and the average value is calculated in mg / s.
[0150] Oil leakage test method: Use a cigarette cartridge with an atomizer core installed, put it into a special cigarette cartridge oil leakage tester, set the negative pressure to 40Mpa, and observe whether the oil leaks from the cigarette cartridge for 8 hours;
[0151] Table 1
[0152]
[0153] In summary, compared with the prior art, the present application can not only increase the aperture of the first guide hole 103, but also maintain the strength of the ceramic aerogel component 100, achieving a balance between the two, and having obvious cost advantages and quality advantages. The above-mentioned aerogel atomization core 10 can be processed by laser to prepare through holes or blind holes on the existing porous ceramic material, and then prepare a filling component 200 in the through hole or blind hole, such as in-situ growth of SiC nanowires and / or Si3N4 nanowires, so as to increase the filling component 200 without reducing the strength of the porous ceramic material too much, and set the porosity and aperture of the filling component 200 to be larger than the ceramic aerogel component 100, thereby increasing the overall average aperture of the aerogel atomization core 10, thereby solving the contradiction between the aperture size of the aerogel atomization core 10 for electronic cigarettes and the strength of the aerogel atomization core 10 in the traditional technology, and improving the service life of the aerogel atomization core 10. Furthermore, the SiC nanowires and / or Si3N4 nanowires grown in the present application will not cause the electronic cigarette cartridge to leak oil, thereby reducing production costs and avoiding possible impacts on the atomization effect.
[0154] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0155] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0156] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An aerogel atomization core, characterized in that: The invention comprises a ceramic aerogel component, a filling component and a heating component, wherein the ceramic aerogel component comprises a first surface and a second surface arranged at relative positions, the ceramic aerogel component is provided with a first guide hole extending from the first surface to the second surface, the filling component is filled in the first guide hole, the porosity of the filling component is greater than the porosity of the ceramic aerogel component and / or the pore size of the filling component is greater than the pore size of the ceramic aerogel component, and the heating component is connected to the second surface.
2. The aerogel atomization core according to claim 1, characterized in that: The first guide hole is a blind hole, which opens on the first surface. The depth of the blind hole extending from the first surface to the second surface is 1 mm to 3 mm.
3. The aerogel atomization core according to claim 1, characterized in that: The first guide hole is a through hole, one end of the first guide hole opens to the first surface and the other end of the first guide hole opens to the second surface.
4. The aerogel atomization core according to claim 1, characterized in that: The aerogel atomization core meets at least one of the following conditions: (1) There are a plurality of first guide holes, the plurality of first guide holes are spaced apart, and each first guide hole is filled with the filling component; the first guide hole is a cylindrical hole, and the hole diameter of the first guide hole is 0.1 mm to 1 mm; (2) The filling components include but are not limited to SiC nanowires and / or Si3N4 nanowires; (3) A second guide hole is also provided on the ceramic aerogel component, and the aperture of the second guide hole is 0.001 mm to 0.15 mm; (4) The preparation material of the ceramic aerogel component includes one or more of a carbon source, a nitrogen source and a silicon source; (5) The porosity of the ceramic aerogel component is 50% to 90%; (6) The pore size of the ceramic aerogel component is 0.5 μm-60 μm; (7) The porosity of the filling component is 60%-90%; (8) The pore size of the filling component is 1 μm to 80 μm.
5. The aerogel atomization core according to any one of claims 1 to 4, characterized in that: An oil storage tank is provided on the first surface of the ceramic aerogel component, and the depth of the oil storage tank is 1 mm to 1.6 mm. When the first guide hole is a through hole, the two ends of the first guide hole are respectively opened to the bottom surface of the oil storage tank and the second surface. When the first guide hole is a blind hole, the first guide hole is opened to the bottom surface of the oil storage tank.
6. A method for preparing the aerogel atomization core according to any one of claims 1 to 5, characterized in that: The steps include: Preparing a first guide hole on the ceramic aerogel component, wherein the first guide hole extends from the first surface to the second surface of the ceramic aerogel component; preparing a filling component in the first guide hole, wherein the porosity of the filling component is greater than the porosity of the ceramic aerogel component and / or the pore size of the filling component is greater than the pore size of the ceramic aerogel component; and A heating component is connected to the second surface of the ceramic aerogel component to obtain an aerogel atomization core.
7. The method for preparing an aerogel atomization core according to claim 6, characterized in that: When preparing the first guide hole on the ceramic aerogel component, the following steps are included: The green body required for preparing the ceramic aerogel component is placed in a laser and mechanical processing device, and a through hole and / or a blind hole with a diameter of 0.1 mm to 1 mm is prepared on the green body as a first guide hole.
8. The method for preparing the aerogel atomization core according to claim 6 or 7, characterized in that: The preparation method of the aerogel atomization core meets at least one of the following conditions: (1) When preparing a filling component in the first guide hole, the following steps are included: Putting the green body with the first guide hole into a sintering furnace to in-situ grow SiC nanowires and / or Si3N4 nanowires, setting the temperature to 1000°C to 1800°C, the time to 1h to 8h, the pressure to 0.01MPa to 1MPa, introducing argon or nitrogen, the diameters of the SiC nanowires and / or Si3N4 nanowires are 5nm to 200nm respectively; (2) The method for preparing the aerogel atomizer core further comprises the following step: subjecting the prepared aerogel atomizer core to high temperature treatment.
9. An atomizer, characterized in that: The invention comprises the aerogel atomization core as described in any one of claims 1 to 6, or the aerogel atomization core prepared by the preparation method as described in any one of claims 6 to 8.
10. An electronic atomization device, characterized in that: The invention comprises the atomizer as claimed in claim 9 and a power supply component, wherein the power supply component is electrically connected to a heating component of the aerogel atomization core in the atomizer.
Citation Information
Patent Citations
Atomizing core, electronic cigarette and manufacturing method of atomizing core
CN113768192A
Atomizing core, atomizer, aerosol generating device and atomizing core processing method
CN115918976A
Large-aperture high-strength ceramic atomizing core and preparation method thereof
CN116098320A
Electronic cigarette atomization core and electronic cigarette