Ag / ZnO / MXene fabric-based photocatalytic composite material as well as preparation method and application thereof
By loading silver nanoparticles on ZnO/MXene fabrics, Ag/ZnO/MXene fabric-based composite photocatalytic materials are prepared, which solves the problems of low efficiency and difficulty in recycling of existing photocatalysts, and achieves efficient wastewater treatment and UV resistance.
Patent Information
- Application Number
- CN202410919087.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
Existing photocatalytic fabrics are inefficient when degrading wastewater pollutants and are difficult to recycle, have low photoenergy utilization, and the aggregation of titanium dioxide affects the specific surface area and catalytic performance.
Using ZnO/MXene functional fabric as a support, silver nanoparticles are loaded on ZnO/MXene fabric with dopamine, and Ag/ZnO/MXene fabric-based composite photocatalytic material is prepared through oscillation and washing processes to improve photocatalytic efficiency and realize the material Reused.
The photocatalytic efficiency of the photocatalyst is significantly improved, the light absorption capacity and electron transfer rate are enhanced, the wastewater treatment efficiency is improved, and the reuse of materials and ultraviolet resistance are achieved.
Smart Images

Figure BDA0004936072060000121 
Figure HDA0004936072070000011 
Figure HDA0004936072070000012
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to functional textile materials, and more specifically, relates to an Ag / ZnO / MXene fabric-based photocatalytic composite material and a preparation method and application thereof. Background Art
[0002] In the context of a dual-carbon world, effective water pollution control has become a new challenge for all countries. As a major textile printing and dyeing industry country, printing and dyeing wastewater has become a prominent problem in my country's environmental governance due to the wide variety of dyes and complex compositions. Photocatalytic treatment of printing and dyeing wastewater is one of the most effective and inexpensive methods, which allows the complete mineralization of these environmentally harmful dyes. In addition, photocatalytic degradation has the advantages of being non-toxic, low in energy consumption, easy to operate, mild in reaction conditions, and can effectively remove organic pollutants in wastewater. It has great advantages in dye wastewater treatment. There are many types of materials with photocatalytic reaction mechanisms in the prior art, and the catalytic efficiency and durability of the catalytic materials are generally pursued in the industry.
[0003] At present, some progress has been made in the research of composite photocatalytic fabrics, among which the representative ones include graphene / titanium dioxide composite fabrics. This composite fabric is prepared by combining graphene with titanium dioxide using sol-gel method and other methods. The introduction of graphene improves the effective absorption of titanium dioxide to visible light, so that the composite fabric shows good photocatalytic activity for organic pollutants such as active red dye under sunlight conditions. Although the graphene / titanium dioxide composite fabric has excellent photocatalytic performance, it still has the problem of low light energy utilization. Titanium dioxide (anatase type) has a wide bandgap and only responds to ultraviolet light, while ultraviolet light accounts for only about 4% of the solar spectrum, resulting in most of the visible light cannot be effectively utilized. During the preparation process, nano-scale titanium dioxide is very easy to agglomerate, which makes its specific surface area smaller and cannot fully contact with pollutants, thereby affecting the performance of photocatalysis. Moreover, after the photogenerated electrons and holes are excited, their transfer rate is slow and partially recombine, which greatly reduces the efficiency of photocatalysis.
[0004] Doping precious metals with photocatalysts is one of the effective methods for improving photocatalysts. Silver nanoparticles are a common metal co-catalyst with strong surface plasmon resonance, good visible light transmittance and large specific surface area, but whether they can be combined with precious metals for use in textile-based materials and as catalytic materials has been rarely studied. Summary of the invention
[0005] In view of the above defects or improvement needs of the prior art, the present invention provides an Ag / ZnO / MXene fabric-based photocatalytic composite material and a preparation method and application thereof. The purpose of the method is to prepare an Ag / ZnO / MXene fabric-based composite photocatalytic material by using ZnO / MXene functional fabric as a carrier and utilizing the reducing property of dopamine to load silver nanoparticles on the ZnO / MXene fabric, thereby improving the photocatalytic efficiency of the composite photocatalytic material, thereby solving the problem of low efficiency of traditional photocatalysts in degrading wastewater pollutants. At the same time, the prepared composite material can be recycled and reused after treating sewage.
[0006] To achieve the above object, according to one aspect of the present invention, a method for preparing a Ag / ZnO / MXene fabric-based photocatalytic composite material is provided, comprising the following steps:
[0007] The ZnO / MXene functional fabric is immersed in a first dopamine solution and shaken, reacted, and washed, and then the obtained fabric is added to a silver nitrate solution, shaken, reacted, washed, and dried to obtain a Ag / ZnO / MXene fabric-based photocatalytic composite material;
[0008] It should be noted that oscillation and washing in the above reaction process are conventional means. For example, the purpose of oscillation is to increase the contact between the functional substances in the solution and the substrate and improve the reaction efficiency. This can also be achieved by means such as stirring.
[0009] Wherein, the first dopamine solution is a dopamine Tris-HCl solution, and the dosage of dopamine is 1-4 g / L;
[0010] The pH range in Tris-HCl buffer was 8.5 ± 0.2;
[0011] The Tris-HCl buffer solution is prepared by first preparing a solution with a Tris concentration of 10 mM, and then adjusting the pH of the solution to 8.5±0.2 using HCl;
[0012] Further, the ZnO / MXene functional fabric is immersed in the first dopamine solution and shaken. The bath ratio of the ZnO / MXene functional fabric to the first dopamine solution is 1:50-300; the preferred bath ratio is 1:50-200; and the more preferred bath ratio is 1:100-120;
[0013] The ZnO / MXene functional fabric is immersed in the first dopamine solution and shaken for 1-4 h.
[0014] Furthermore, the concentration of the silver nitrate solution is 1-10 mM;
[0015] Furthermore, the bath ratio of the ZnO / MXene functional fabric to the silver nitrate solution is 1:50-300; the preferred bath ratio is 1:50-200; and the more preferred bath ratio is 1:100-120.
[0016] The obtained fabric is added into the silver nitrate solution and the shaking reaction time is 30-180 minutes.
[0017] In some embodiments, the ZnO / MXene functional fabric used in the present invention is prepared by the following method: zinc acetate and sodium hydroxide solids are mixed and added to water to obtain a mixed solution, the mixed solution is diluted, and then multilayer MXene powder is added, mixed and stirred to obtain a ZnO / MXene mixed solution;
[0018] The fabric is placed in the ZnO / MXene mixed solution and stirred to react, and then washed and dried to obtain the ZnO / MXene functional fabric.
[0019] Wherein, the fabric may be a polydopamine fabric, and the polydopamine fabric is a fabric treated with polydopamine;
[0020] The preparation method of the polydopamine fabric comprises the following steps: adding dopamine to a Tris-HCl buffer solution to obtain a second dopamine solution, placing the fabric in the dopamine solution for immersion and shaking, and then washing and drying to obtain the polydopamine fabric.
[0021] Furthermore, the preparation method of the polydopamine fabric is to add dopamine to a Tris-HCl buffer solution to obtain a second dopamine solution, wherein the concentration of dopamine in the second dopamine solution is 1-5 g / L, preferably 2-4 g / L, and more preferably 5 g / L;
[0022] Further, zinc acetate and sodium hydroxide solid are mixed and added to water to obtain a mixed solution, wherein the zinc acetate concentration in the solution is 0.5-1.5M, and preferably the zinc acetate concentration is 1M.
[0023] The sodium hydroxide concentration is 7-8M; the preferred sodium hydroxide concentration is 8M
[0024] Further, adding to water to obtain a mixed solution, the mixed solution is diluted, wherein the dilution multiple is 15-35 times, and the preferred dilution multiple is 18-25 times;
[0025] Further, multilayer MXene powder is added, wherein the multilayer MXene powder is added to the diluted mixed solution at a concentration of 2-10 mg / mL; preferably, the multilayer MXene concentration is 3-8 mg / mL;
[0026] Furthermore, the mixing and stirring time is 10-50 minutes.
[0027] The fabric is placed in the second dopamine solution for immersion and shaking, wherein the bath ratio of the fabric to the second dopamine solution is 1:20-300.
[0028] According to another aspect of the present invention, a method for preparing an Ag / ZnO / MXene fabric-based photocatalytic composite material is provided, wherein the Ag / ZnO / MXene fabric-based photocatalytic composite material is prepared using the above method.
[0029] According to another aspect of the present invention, there is provided an application of the Ag / ZnO / MXene fabric-based photocatalytic composite material as described in another aspect of the present invention in sewage treatment and in anti-ultraviolet materials.
[0030] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art:
[0031] The present invention uses fabric as a carrier, and uses the reducing property of dopamine to load Ag nanoparticles on ZnO / MXene fabric to prepare Ag / ZnO / MXene fabric-based composite photocatalytic materials. The composite of multilayer MXene and ZnO helps to shorten the band gap of a single ZnO photocatalyst, enhance its light absorption capacity, promote the transfer of photogenerated electron-hole pairs, and improve its photocatalytic activity. The doping of Ag nanoparticles can not only promote the photocatalyst to produce more free radicals to participate in the photocatalytic oxidation process, but also help to enhance the oxidation ability of electrons on the conduction band of the ZnO / MXene fabric photocatalytic material and improve its photocatalytic activity. At the same time, in order to solve the problem that traditional photocatalysts are difficult to recycle and process when degrading wastewater pollutants, the present invention uses fabric as a carrier and uses the adhesion of polydopamine to synthesize Ag / ZnO / MXene fabric-based composite photocatalytic materials on a cotton substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a SEM image of the Ag / ZnO / MXene fabric-based composite photocatalytic material exemplified in Example 1 of the present invention;
[0033] Figure 2 is the absorbance of the Ag / ZnO / MXene fabric-based composite photocatalytic material used in Example 1 of the present invention to degrade methylene blue dye;
[0034] Figure 3 is the efficiency of the Ag / ZnO / MXene fabric-based composite photocatalytic material in Example 1 of the present invention in degrading methylene blue dye;
[0035] Figure 4It is the efficiency of degrading methylene blue dye by repeatedly using the Ag / ZnO / MXene fabric-based composite photocatalytic material for three times in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0037] The present invention provides a method for preparing a Ag / ZnO / MXene fabric-based photocatalytic composite material, which specifically comprises the following steps:
[0038] The ZnO / MXene functional fabric is immersed in a first dopamine solution and shaken, reacted, and washed, and then the obtained fabric is added to a silver nitrate solution, shaken, reacted, washed, and dried to obtain a Ag / ZnO / MXene fabric-based photocatalytic composite material;
[0039] Wherein, the first dopamine solution is a dopamine Tris-HCl solution, and the amount of dopamine used is 1-4 g / L; for example, the dopamine content can be 1 g / L, 2 g / L, or 4 g / L;
[0040] The pH range in Tris-HCl buffer was 8.5 ± 0.2;
[0041] The Tris-HCl buffer solution is prepared by first preparing a solution with a Tris concentration of 10 mM, and then adjusting the pH of the solution to 8.5±0.2 using HCl;
[0042] Further, the ZnO / MXene functional fabric is immersed in the first dopamine solution and shaken. The bath ratio of the ZnO / MXene functional fabric to the first dopamine solution is 1:50-300; the preferred bath ratio is 1:50-200; and the more preferred bath ratio is 1:100-120;
[0043] The ZnO / MXene functional fabric is immersed in the first dopamine solution and shaken for a shaking time of 1-4 hours, for example, the shaking time is 1 hour, 2 hours, and 4 hours;
[0044] Further, the concentration of the silver nitrate solution is 1-10 mM; for example, the concentration of the silver nitrate solution can be 1 mM, 3 mM, 5 mM, 8 mM or 10 mM;
[0045] Furthermore, the bath ratio of the ZnO / MXene functional fabric to the silver nitrate solution is 1:50-300; the preferred bath ratio is 1:50-200; and the more preferred bath ratio is 1:100-120.
[0046] After the fabric is added to the silver nitrate solution, the shaking reaction time is 30-180 minutes.
[0047] The present invention prepares an Ag / ZnO / MXene fabric-based photocatalytic composite material by adsorbing a layer of dopamine on a ZnO / MXene functional fabric, adding the dopamine-adsorbed functional fabric into a silver nitrate solution, and using the reducing property of dopamine to load Ag nanoparticles on the ZnO / MXene fabric, thereby preparing an Ag / ZnO / MXene fabric-based composite photocatalytic material.
[0048] In some embodiments, the ZnO / MXene functional fabric used in the present invention is prepared by the following method: zinc acetate and sodium hydroxide solids are mixed and added to water to obtain a mixed solution, the mixed solution is diluted, and then multilayer MXene powder is added, mixed and stirred to obtain a ZnO / MXene mixed solution;
[0049] The fabric is placed in the ZnO / MXene mixed solution and stirred to react, and then washed and dried to obtain the ZnO / MXene functional fabric.
[0050] Zinc acetate and sodium hydroxide solid are mixed, wherein the solid state can be in the form of flakes or powder;
[0051] Zinc acetate and sodium oxide are mixed and added to water to obtain a mixed solution, wherein the concentration of zinc acetate in the solution is 0.5-1.5 M, for example, 0.5 M, 1 M, or 1.5 M;
[0052] The sodium hydroxide concentration is 7-8M; for example, the sodium hydroxide concentration is 7M, 8M;
[0053] The mixed solution is diluted by 15-35 times, such as 15 times, 20 times, and 35 times;
[0054] The multi-layer MXene powder is added to the diluted mixed solution at a concentration of 2-10 mg / mL; for example, the concentration may be 3 mg / mL, 5 mg / mL, or 8 mg / mL.
[0055] Placing the fabric in the ZnO / MXene mixed solution and stirring, wherein the bath ratio of the fabric to the ZnO / MXene mixed solution is 1:20-300, for example, the bath ratio may be 1:50, 1:100, 1:200;
[0056] In some embodiments, the fabric in the ZnO / MXene functional fabric is a polydopamine fabric, and the polydopamine fabric is a fabric treated with polydopamine;
[0057] The preparation method of the polydopamine fabric comprises the following steps: adding dopamine to a Tris-HCl buffer solution to obtain a second dopamine solution, placing the fabric in the dopamine solution for immersion and shaking, and then washing and drying to obtain the polydopamine fabric.
[0058] Furthermore, the preparation method of the polydopamine fabric is to add dopamine to a Tris-HCl buffer solution to obtain a second dopamine solution, wherein the concentration of dopamine in the second dopamine solution is 1-5 g / L, preferably 2-4 g / L, and more preferably 5 g / L;
[0059] The fabric is placed in the second dopamine solution for immersion and shaking, wherein the bath ratio of the fabric to the second dopamine solution is 1:20-300.
[0060] In addition, the present invention also provides a method for preparing multilayer MXene: slowly adding titanium aluminum carbide powder to a mixed solution of lithium fluoride powder and hydrochloric acid, stirring the mixture to react, and then acid-washing, centrifuging multiple times, and freeze-drying the resulting reaction solution to obtain the multilayer MXene powder required for the experiment;
[0061] Specifically, the present invention provides the following embodiments:
[0062] Example 1 Preparation of multilayer MXene,
[0063] In the preparation of multilayer MXene, the hydrochloric acid concentration is 10M, the hydrochloric acid is 30ml, the lithium fluoride (LiF) powder is 1.5g, the titanium aluminum carbide (Ti3AlC2) powder is 1.5g, the reaction temperature is 40°C, the reaction time is 36h, the stirring speed is 540rpm, the hydrochloric acid concentration used for pickling is 1M, the number of pickling times is 3 times, the centrifugal speed is 3500rpm, the single centrifugation time is 5min, the pH test paper is used to test the supernatant after centrifugation to be greater than 6 and then the centrifugation is stopped, and the freeze-drying time is 12h.
[0064] Example 2 Preparation of ZnO / MXene mixed solution
[0065] In the preparation of the ZnO / MXene mixed solution, the zinc acetate concentration was 1 M, the sodium hydroxide concentration was 8 M, the MXene concentration was 5 mg / mL, the zinc acetate and sodium hydroxide dilution multiples were 20 times, and the stirring time after mixing was 30 min.
[0066] Specifically, 2.19 g of zinc acetate powder and 3.28 g of sodium hydroxide powder were respectively put into 2 ml of deionized water, and after dissolution, the two were mixed and diluted to 20 times with deionized water. After stirring for 30 minutes, 0.2 g of MXene powder was added to prepare a ZnO / MXene mixed solution.
[0067] Example 3 Preparation of polydopamine fabric
[0068] In the preparation of polydopamine fabric, the Tris concentration in the Tris-HCl buffer was 10 mM, and then HCl was used to adjust the pH to 8.5±0.2. The concentration of dopamine was 4 g / L, and the shaking was performed for 1 hour at room temperature with a shaking speed of 100 rpm. The washing and drying was performed by washing with distilled water 2-3 times and drying at 30°C.
[0069] Example 4 Preparation of ZnO / MXene functional fabric
[0070] In the preparation of ZnO / MXene functional fabrics, the polydopamine fabric prepared in Example 3 was added to the ZnO / MXene mixed solution prepared in Example 2, the stirring time was 8 hours, the drying temperature was 60°C, and the drying time was 30 minutes, wherein the bath ratio of the fabric in Example 3 to the ZnO / MXene mixed solution was 1:100.
[0071] Example 5 Preparation of ZnO / MXene functional fabric
[0072] The scheme is based on Example 4, except that the fabric used is not treated by Example 3, that is, conventional fabric is added to the ZnO / MXene mixed solution prepared in Example 2, the stirring time is 8 hours, the drying temperature is 60°C, and the drying time is 30 minutes, wherein the bath ratio of the fabric in Example 3 to the ZnO / MXene mixed solution is 1:100.
[0073] Example 6 Preparation of Ag / ZnO / MXene fabric-based composite photocatalytic material
[0074] In the preparation of Ag / ZnO / MXene fabric-based composite photocatalytic material, the ZnO / MXene functional fabric prepared in Example 4 is immersed in the first dopamine solution and shaken, reacted, washed, and then the obtained fabric is added to the silver nitrate solution, shaken, reacted, washed and dried to obtain the Ag / ZnO / MXene fabric-based photocatalytic composite material; in the Tris-HCl buffer, the Tris concentration is 10mM, and then HCl is used to adjust the pH to 8.5±0.2. For example, the concentration of dopamine is 2g / L, the concentration of the silver nitrate solution is 5mM, the third shaking is shaking at room temperature for 1h, the shaking speed is 100rpm, and the washing and drying is washing with distilled water 2-3 times and drying at 30°C. The bath ratio of the ZnO / MXene functional fabric to the first dopamine solution is 1:100.
[0075] Example 7 Preparation of Ag / ZnO / MXene fabric-based composite photocatalytic material
[0076] The operation is based on Example 6, except that the ZnO / MXene functional fabric prepared in Example 5 is immersed in the first dopamine solution and shaken, reacted, and washed, and then the obtained fabric is added to a silver nitrate solution, shaken, reacted, washed and dried to obtain an Ag / ZnO / MXene fabric-based photocatalytic composite material.
[0077] In this preparation process, dopamine is used twice, but for different purposes. First, the preparation of polydopamine fabric (see Example 3), in which dopamine mainly plays an adhesion role. Dopamine forms a dense polydopamine film on the surface of the fabric, which has strong adhesion and promotes the bonding of ZnO / MXene to the fabric.
[0078] Dopamine used in the preparation of Ag / ZnO / MXene fabric-based composite photocatalytic materials plays a reducing role. The reducing property of dopamine is used to load Ag nanoparticles on ZnO / MXene fabric to prepare Ag / ZnO / MXene fabric-based composite photocatalytic materials.
[0079] For comparative example 1, refer to Example 1 of a method for preparing a MXene functional cotton fabric disclosed in the previous application of this research group with publication number CN116536916A. The MXene used in this example is the same as that prepared in this application.
[0080] At the same time, referring to the test method provided in the previous application publication number CN116536916A of this subject, the photocatalytic performance of the Ag / ZnO / MXene fabric-based composite photocatalytic material prepared by the present invention is characterized by degrading methylene blue (MB) under full light irradiation. 100mL of methylene blue (MB) solution was added to a glass reaction container, and then the Ag / ZnO / MXene fabric-based composite photocatalytic material was immersed in the methylene blue (MB) solution. The initial concentration of the methylene blue solution was 10mg / L, and the bath ratio of the fabric-based photocatalytic composite material to the methylene blue solution was 1:100. Before irradiation, it was first stirred for 30min under dark conditions. After the catalyst and the dye reached adsorption-desorption equilibrium, the GEL-HXUV300 xenon lamp light source was turned on to carry out the photocatalytic reaction. After irradiation, samples were taken every 20min, and the absorbance of the residual dye in the solution was determined by a SPECORD@210PLUS ultraviolet-visible photometer, and then the degradation rate of the dye was calculated according to the change in the absorbance of the solution.
[0081] Degradation rate (%) = (C0-C t ) / C t =(A0-A t ) / A t
[0082] C0: initial concentration of dye solution; C t is the concentration of the fuel solution at the time of illumination t; A0 is the initial absorbance of the dye solution, A t is the absorbance of the fuel solution at time t after illumination;
[0083] Repeatable photocatalytic performance test (durability), the Ag / ZnO / MXene fabric-based composite photocatalytic material for photocatalytic degradation of methylene blue was taken out from the dye solution, dried in an oven at 60°C, and then added to 100ml of dye solution, the initial concentration of the dye methylene blue was 10mg / L. Before irradiation, it was first stirred for 30min under dark conditions. After the catalyst and dye reached adsorption-desorption equilibrium, the GEL-HXUV300 xenon lamp light source was turned on for photocatalytic reaction. After irradiation, samples were taken every 20min, and the absorbance of the residual dye in the solution was measured with a SPECORD@210PLUS UV-visible photometer, and then the degradation rate of the dye was calculated based on the change in the absorbance of the solution.
[0084] The photocatalytic activity of Ag / ZnO / MXene fabric-based composite photocatalysts was evaluated by degrading methylene blue (MB) under full light irradiation.
[0085] See also Figure 1, which characterizes the scanning electron microscope image of the Ag / ZnO / MXene fabric-based composite photocatalytic material prepared in Example 7. It can be seen that a large number of tiny particles are attached to the surface of the prepared photocatalytic material fiber, and compared with the MXene functional cotton fabric prepared in Comparative Example 1, the fine particles are evenly dispersed. At the same time, the distribution of fine particles can be clearly seen on the multi-layer MXene structure, and the fine particles are reduced silver particles or zinc oxide particles.
[0086] like Figure 2 As shown in Example 7, the absorbance of the MB solution at 664 nm of the Ag / ZnO / MXene fabric-based composite photocatalytic material prepared by the irradiation time increases, and the color decreases significantly after the start of irradiation; it almost disappears after 80 minutes of irradiation.
[0087] Figure 3 The variation of MB concentration (C / C0) with reaction time during the photocatalytic reduction process is described, wherein C and C0 represent the concentration and initial concentration of methylene blue, respectively. The results show that 91.6% of MB is degraded under full light irradiation for 80 minutes, indicating that the prepared photocatalyst has high photocatalytic activity in MB degradation. From the perspective of photocatalytic degradation rate, at the beginning of illumination, the decrease in its absorbance is significantly higher than that of the functional fabric prepared in the embodiment of Comparative Example 1. Within 40 minutes after illumination, the degradation rate of the material in Comparative Example 1 decreases by about 47%, while the degradation rate of the fabric-based composite photocatalytic material in Example 7 of the present invention reaches 65%, which is significantly better than the material provided in Comparative Example 1.
[0088] Figure 4 It shows that after three repeated cycles, the photocatalytic degradation rate of MB did not decrease significantly, indicating that an Ag / ZnO / MXene fabric-based composite photocatalytic material has good photocatalytic degradation cycle stability.
[0089] Based on the Ag / ZnO / MXene fabric-based photocatalytic composite material obtained in Example 1, its anti-ultraviolet performance is applied.
[0090] The UV protection factor (UPF) is used to analyze the ultraviolet protection ability of the fabric, and the UPF value of the Ag / ZnO / MXene fabric-based composite photocatalytic material is shown in Table 1. As can be seen from the table, the UPF value of the original fabric is 16, and it has no anti-ultraviolet performance, while the UPF value of the treated functional fabric is much greater than 50 (GB / T18830-2009), and T (UVA) = 0.05%, which shows that the Ag / ZnO / MXene fabric-based composite photocatalytic material has good anti-ultraviolet performance.
[0091] Table 1 Comparison of UV resistance of original fabric and Ag / ZnO / MXene fabric-based composite photocatalytic materials
[0092]
[0093] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a Ag / ZnO / MXene fabric-based photocatalytic composite material, characterized in that: The steps include: The ZnO / MXene functional fabric is immersed in a first dopamine solution and oscillated to react, and the dopamine-attached fabric is added to a silver nitrate solution and oscillated to react to obtain an Ag / ZnO / MXene fabric-based photocatalytic composite material.
2. The method for preparing the Ag / ZnO / MXene fabric-based photocatalytic composite material according to claim 1, characterized in that: The first dopamine solution is a dopamine Tris-HCl solution, wherein the dopamine concentration is 1-4 g / L.
3. The method for preparing the Ag / ZnO / MXene fabric-based photocatalytic composite material according to claim 1, characterized in that: The preparation method of the ZnO / MXene functional fabric is: Mix zinc acetate and sodium hydroxide solids, add them to water to obtain a mixed solution, dilute the mixed solution, then add multilayer MXene powder, mix and stir to obtain a ZnO / MXene mixed solution; The fabric is placed in the ZnO / MXene mixed solution and stirred, and the ZnO / MXene functional fabric is obtained after reaction.
4. The method for preparing the Ag / ZnO / MXene fabric-based photocatalytic composite material according to claim 3, characterized in that: The fabric is a polydopamine fabric, and the polydopamine fabric is a fabric treated with polydopamine; The preparation method of the polydopamine fabric comprises the following steps: adding dopamine to a Tris-HCl buffer solution to obtain a second dopamine solution, placing the fabric in the dopamine solution for immersion and shaking, and then washing and drying to obtain the polydopamine fabric.
5. The method for preparing the Ag / ZnO / MXene fabric-based photocatalytic composite material according to claim 4, characterized in that: The preparation method of the polydopamine fabric is to add dopamine into a Tris-HCl buffer solution to obtain a second dopamine solution, wherein the concentration of dopamine in the dopamine solution is 1-5 g / L.
6. The method for preparing the Ag / ZnO / MXene fabric-based photocatalytic composite material according to claim 5, characterized in that: Zinc acetate and sodium hydroxide solids are mixed and added to water to obtain a mixed solution, wherein the concentration of zinc acetate in the solution is 0.5-1.5M, and the concentration of sodium hydroxide is 7-8M; The dilution multiple of the mixed solution is 15-35 times.
7. The method for preparing the Ag / ZnO / MXene fabric-based photocatalytic composite material according to claim 6, characterized in that: The multilayer MXene powder is added, wherein the multilayer MXene powder is added to the diluted mixed solution at a concentration of 2-10 mg / mL; The mixing and stirring time is 10-50 min.
8. The method for preparing the Ag / ZnO / MXene fabric-based photocatalytic composite material according to claim 7, characterized in that: The fabric is placed in the second dopamine solution for immersion and shaking, wherein the bath ratio of the fabric to the second dopamine solution is 1:20-300.
9. The method for preparing the ZnO / MXene fabric-based photocatalytic composite material according to any one of claims 1 to 8, characterized in that: Immersing the ZnO / MXene functional fabric in the first dopamine solution and shaking the ZnO / MXene functional fabric to the first dopamine solution in a bath ratio of 1:50-300; The concentration of silver nitrate solution is 1-10mM; The reaction time is 6-12h; the drying temperature is 50-80°C.
10. An Ag / ZnO / MXene fabric-based photocatalytic composite material obtained by the preparation method of the Ag / ZnO / MXene fabric-based photocatalytic composite material according to any one of claims 1 to 8.
Citation Information
Patent Citations
Preparation method of dopamine modified nano-silver textile fabric
CN105442306A
Antibacterial fabric preparation process
CN107227610A
Fabric-based Ag / ZIF-8 functional material as well as preparation method and application thereof
CN115739183A
Fabric-based silver / titanium dioxide functional material and preparation method thereof
CN115957814A
MXene functional cotton fabric as well as preparation method and application thereof
CN116536916A
Cited By
Porous titanium-based implant with photo-thermal surface as well as preparation method and application of porous titanium-based implant
CN120586149A