Anti-carbon-deposition nickel-based catalyst for methane and carbon dioxide dry reforming as well as preparation method and application of anti-carbon-deposition nickel-based catalyst
By using a cerium-based MOF template to prepare an anti-carbon deposit nickel-based catalyst for CeO2 nanotube support, doping Zr to form a solid solution, solving the problem of carbon deposit deactivation and short service life of the nickel-based catalyst in the methane carbon dioxide dry reforming reaction. The catalyst is efficient and stable and has good carbon deposit resistance.
Patent Information
- Application Number
- CN202410772495.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-11-08
AI Technical Summary
In the methane carbon dioxide dry reforming reaction, the nickel-based catalyst is prone to carbon deposits, resulting in inactivation, and the conversion temperature is high and the service life is not long. The existing supported non-precious metal nickel-based catalysts have insufficient carbon deposit resistance.
Thin-walled nanotube precursors were prepared using cerium-based MOF templates, and anti-carbon deposit nickel-based catalysts were prepared by immersion, drying, calcining and reducing treatments. CeO2 nanotubes were used as support and doped with Zr to form solid solution to improve the resistance of the catalyst. Carbon deposit performance.
The resistance to carbon deposits of the catalyst was significantly improved. The amount of carbon deposits in the 100h test did not increase significantly compared with that in the 10h test. The catalytic activity was highly maintained, and the conversion rate of carbon dioxide and methane remained at 90% or above, which solved the problem of nickel-based catalysts. High conversion temperature and carbon deposition inactivation.
Smart Images

Figure CN118904347A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of dry reforming, and in particular to a carbon deposition resistant nickel-based catalyst for dry reforming of methane and carbon dioxide, a preparation method and application thereof. Background Art
[0002] Methane CO2 dry reforming (DRM), also known as methane dry reforming reaction, uses two greenhouse gases, CO2 and CH4, to produce synthesis gas. It has the dual advantages of mitigating the greenhouse effect and providing high-value chemical raw materials, and will play an important role in future energy structure and carbon emission reduction. Thermodynamically, due to the side reactions of CH4 cracking and CO disproportionation, the DRM reaction easily forms a large amount of carbon deposits in the range of 550-700°C, which deactivates the catalyst. Therefore, in the low-temperature (such as 550°C) DRM process that is very likely to cause serious thermodynamic carbon deposition, it is crucial to design a catalyst to balance the kinetics between carbon formation and carbon removal to achieve good catalytic activity and long-term stability.
[0003] In recent years, people have devoted themselves to the development of excellent catalysts for DRM reactions, especially non-precious metal Ni-based catalysts, which have catalytic activities comparable to those of precious metals such as Pt and Rh. However, the severe carbon deposition caused by the imbalanced kinetics between rapid carbon formation and slow carbon removal still limits the application of this catalyst in DRM reactions. In order to improve its anti-carbon deposition performance, the DRM performance of supported non-precious metal nickel-based catalysts prepared with Al2O3, SiO2, ZrO2 and MgO as carriers in the prior art has been widely explored, but there are still common problems such as high conversion temperature, easy carbon deposition and deactivation, and short service life. Therefore, it is necessary to develop new strategies to design supported nickel-based catalysts with high carbon deposition resistance for methane carbon dioxide dry reforming. Summary of the invention
[0004] In view of the above problems, the present invention provides a carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming, a preparation method and an application thereof. The carbon deposition resistant nickel-based catalyst is prepared by combining the improvement of the formula and the process, and is made to have excellent carbon deposition resistance, so as to solve the problems of high conversion temperature and carbon deposition deactivation of nickel-based catalysts in the methane carbon dioxide dry reforming reaction.
[0005] The purpose of the present invention is achieved by the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming, comprising the following steps:
[0007] (1) preparing a cerium-based MOF template;
[0008] (2) calcining the cerium-based MOF template to obtain a thin-walled nanotube precursor;
[0009] (3) Using a mixed aqueous solution of nickel salt and zirconium dinitrate hydrate as an impregnation solution, the nanotube precursor is sequentially subjected to impregnation, drying, calcination and reduction treatment to prepare a carbon deposition resistant nickel-based catalyst.
[0010] Preferably, in step (1), the cerium-based MOF template is prepared by a solvent method.
[0011] More preferably, the preparation process of the cerium-based MOF template comprises the following steps:
[0012] The cerium salt and 1,3,5-benzenetricarboxylic acid are dissolved in a mixed solution of anhydrous ethanol and deionized water to react, and after the reaction is completed, the cerium-based MOF template is obtained after separation, precipitation, washing and drying.
[0013] More preferably, the reaction is carried out at a temperature of 25-100° C., a reaction time of 0.5-6 h, a mass of 1,3,5-benzenetricarboxylic acid of 2.10 g, a molar ratio of 1,3,5-benzenetricarboxylic acid to the cerium salt of 0.5-3:1, a volume of deionized water of 55 mL, and a volume ratio of deionized water to anhydrous ethanol of 1:1-8:1.
[0014] Preferably, in step (2), the calcination temperature is 25-900° C., the heating rate is 3-15° C. / min, and the calcination time is 0.5-6 h.
[0015] Preferably, in step (3), the impregnation treatment is carried out by an equal volume impregnation method, wherein the mass percentage of elemental nickel in the obtained carbon deposition resistant nickel-based catalyst to the nanotube precursor is 0.1%-20%.
[0016] Preferably, in step (3), the molar ratio of the element zirconium to the element cerium in the obtained carbon deposition resistant nickel-based catalyst is x:(1-x), wherein x=0.01-0.2.
[0017] Preferably, in step (3), the calcination temperature is 500-900° C. and the calcination time is 1-5 h.
[0018] Preferably, in step (3), the reduction treatment is carried out in a hydrogen atmosphere, the reduction temperature is 500-900° C., the reduction time is 0.5-4 h, and the pure hydrogen flow rate is 10-40 mL / min.
[0019] In a second aspect, the present invention provides a carbon deposition resistant nickel-based catalyst for methane and carbon dioxide dry reforming, wherein the catalyst is prepared by the aforementioned preparation method.
[0020] In a third aspect, the present invention provides an application of a carbon deposition resistant nickel-based catalyst as a catalyst in a methane carbon dioxide dry reforming reaction.
[0021] Preferably, during the application of the anti-carbon deposition nickel-based catalyst, the process conditions for methane dry reforming are: reaction temperature is 400-800°C, reaction pressure is atmospheric pressure, the volume ratio of reaction gas is CO2 / CH4 / N2=1:1:(1-10), and the catalyst dosage is 50-200 mg.
[0022] Preferably, in the methane carbon dioxide dry reforming reaction at a reaction temperature of 550°C, the carbon deposition amount of the anti-carbon deposition nickel-based catalyst obtained by the preparation method is only 6.88% in the 100h performance test, which is not significantly increased compared to the carbon deposition amount of 5.24% in the 10h test, and the catalytic activity is highly maintained, the conversion rate of carbon dioxide is maintained at about 90%, and the conversion rate of methane is maintained at more than 93%.
[0023] The beneficial effects of the present invention are:
[0024] (1) The carbon deposition resistant nickel-based catalyst prepared by the present invention through the combination of formula and process improvement is a newly designed supported high carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming, which has excellent carbon deposition resistance. The carbon deposition amount in the 100h test does not change significantly compared with that in the 10h test, and the catalytic activity is highly maintained, which effectively solves the problems of high conversion temperature and carbon deposition deactivation of nickel-based catalysts in the methane carbon dioxide dry reforming reaction.
[0025] (2) The anti-carbon deposition nickel-based catalyst prepared by the present invention, the CeO2 nanotubes derived from metal organic framework materials (MOFs) have a large cavity and a thin-wall structure, which can evenly anchor the active metal Ni and can easily dope Zr into its lattice to form a solid solution.
[0026] (3) The carbon deposition resistant nickel-based catalyst prepared by the present invention has a higher carbon deposition resistance than Ni / CeO2 in the 10 h test in the methane carbon dioxide dry reforming reaction at 550°C. 0.93 Zr 0.07 O2) has excellent anti-carbon deposition performance. The amount of carbon deposition in the 100h test has no significant change compared with that in the 10h test, and the catalytic activity is highly maintained, which effectively solves the problems of high conversion temperature and carbon deposition deactivation of nickel-based catalysts in the methane carbon dioxide dry reforming reaction.
[0027] (4) The method for preparing the carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming provided by the present invention has a simple process, mild conditions, can be produced on a large scale, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.
[0029] Figure 1 The catalysts prepared in Comparative Example 1 and Example 3 (Ni / CeO2 and Ni / Ce 0.93 Zr 0.07 O2) scanning electron microscope (SEM)-transmission electron microscope (TEM) image;
[0030] Figure 2 is the XRD spectra of the catalysts prepared in Comparative Example 1 and Examples 1-3;
[0031] Figure 3 The catalyst in Comparative Example 1 was heated at a space velocity of 3000 mL·h -1 ·g cat -1 , the performance results of methane carbon dioxide dry reforming reaction at a temperature of 550°C and a reaction time of 10h;
[0032] Figure 4 The results of thermogravimetric (TG-DTG) analysis of the catalysts used in Comparative Example 1 and Examples 1-5 after performance testing;
[0033] Figure 5 The catalyst in Example 1 was heated at a space velocity of 3000 mL·h -1 ·g cat -1 , the performance results of methane carbon dioxide dry reforming reaction at a temperature of 550°C and a reaction time of 10h;
[0034] Figure 6 The catalyst in Example 2 was heated at a space velocity of 3000 mL·h -1 ·g cat -1 , the performance results of methane carbon dioxide dry reforming reaction at a temperature of 550°C and a reaction time of 10h;
[0035] Figure 7 The catalyst in Example 3 was heated at a space velocity of 3000 mL·h -1 ·g cat -1 , the performance results of methane carbon dioxide dry reforming reaction at a temperature of 550°C and a reaction time of 10h;
[0036] Figure 8 The catalyst in Example 4 was heated at a space velocity of 3000 mL·h -1 ·g cat -1, the performance results of methane carbon dioxide dry reforming reaction at a temperature of 550°C and a reaction time of 10h;
[0037] Fig. 9 The catalyst in Example 5 was heated at a space velocity of 3000 mL·h -1 ·g cat -1 , the performance results of methane carbon dioxide dry reforming reaction at a temperature of 550℃ and a reaction time of 100h. DETAILED DESCRIPTION
[0038] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0039] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0040] The present invention is further described below in conjunction with a number of embodiments.
[0041] Example
[0042] The present invention provides a method for preparing a carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming, comprising the following steps:
[0043] (1) preparing a cerium-based MOF template;
[0044] (2) calcining the cerium-based MOF template to obtain a thin-walled nanotube precursor;
[0045] (3) Using a mixed aqueous solution of nickel salt and zirconium dinitrate hydrate as an impregnation solution, the nanotube precursor is sequentially subjected to impregnation, drying, calcination and reduction treatment to prepare a carbon deposition resistant nickel-based catalyst.
[0046] The present invention also provides a carbon deposition resistant nickel-based catalyst for methane and carbon dioxide dry reforming, wherein the catalyst is prepared by the above-mentioned preparation method.
[0047] The present invention also provides an application of a carbon deposition resistant nickel-based catalyst as a catalyst in a methane carbon dioxide dry reforming reaction. During the application of the carbon deposition resistant nickel-based catalyst, the process conditions for methane dry reforming are: a reaction temperature of 400-800°C, a reaction pressure of atmospheric pressure, a reaction gas volume ratio of CO2 / CH4 / N2=1:1:(1-10), and a catalyst dosage of 50-200 mg.
[0048] The following is combined with Figure 1-9 And a plurality of specific embodiments are further described to describe the present invention.
[0049] Example 1
[0050] The anti-carbon deposition nickel-based catalyst, preparation method and application thereof for methane carbon dioxide dry reforming provided in this embodiment are substantially the same as those in the above embodiment, except that the preparation steps are as follows:
[0051] (1) Preparation of Ce-MOF template:
[0052] The Ce-MOF template was prepared by a solvent method. Ce nitrate hexahydrate (4.34 g, 0.01 mol) and 1,3,5-benzenetricarboxylic acid (2.10 g, 0.01 mol) were dissolved in a mixed solution of anhydrous ethanol (10 mL) and deionized water (55 mL). The mixture was stirred at 70 ° C for 1 h to form a precipitate. The product was filtered after cooling to room temperature, washed alternately with deionized water and anhydrous ethanol three times, and dried in a forced air drying oven at 80 ° C overnight. The obtained white precipitate was the Ce-MOF template.
[0053] (2) Preparation of thin-walled CeO2 nanotube precursor:
[0054] The Ce-MOF template was heated to 600° C. in a muffle furnace at a rate of 10° C. / min and calcined for 3 h to obtain a thin-walled CeO2 nanotube precursor;
[0055] Step (3) Weigh 0.051 g of zirconium dinitrate hydrate, and immerse 2.0 g of the nanotube precursor in a mixed aqueous solution of nickel salt and zirconium dinitrate hydrate by an equal volume impregnation method to obtain a Ni / Ce 0.99 Zr 0.01 O2 catalyst, other aspects are the same as those of Comparative Example 1;
[0056] Step (4), the catalyst (Ni / Ce 0.99 Zr 0.01O2) has a Ni loading of 4.88 wt%, and a molar ratio of Zr doped at the Ce site of x=0.01 (i.e., the molar ratio of element zirconium to element cerium is x:(1-x), wherein x=0.01; the description of other embodiments has the same meaning). Figure 2 The XRD analysis results show that compared with the Ni / CeO2 catalyst, Zr doping causes the characteristic diffraction peak of CeO2 crystal surface to move to a higher 2θ direction, and no obvious ZrO2 characteristic diffraction peak is observed, indicating that the Ni / CeO2 0.99 Zr 0.01 The Zr in the O2 catalyst is doped into the CeO2 lattice to form Ce 1-x Zr x O2 solid solution.
[0057] Step (5) using Ni / Ce 0.99 Zr 0.01 O2 catalyst replaced Ni / CeO2 catalyst, and the rest was the same as Comparative Example 1. The test results and TG-DTG analysis of the catalyst used are shown in the attached Figure 5 and Figure 4 From the attached Figure 5 It can be seen that, similar to Comparative Example 1, Ni / Ce 0.99 Zr 0.01 O2 Catalysts X CO2 , X CH4 and R H2 / CO The catalyst also decreased significantly with the extension of reaction time, but the initial CO2 conversion rate was higher and the initial CH4 conversion rate was lower, indicating that Zr doping can promote the activation of CO2 while the activation of CH4 is slightly reduced. Figure 4 It can be seen that the catalyst has a carbon deposition amount of 59.58% in the 10h performance test, and the weight loss peak shifts from 600℃ and 583℃ of the Ni / CeO2 catalyst to a lower 540℃, indicating that the Ni / CeO2 0.99 Zr 0.01 The O2 catalyst has less carbon deposition than the Ni / CeO2 catalyst and the deposited carbon species are easier to eliminate.
[0058] Example 2
[0059] The anti-carbon deposition nickel-based catalyst, preparation method and application thereof for methane carbon dioxide dry reforming provided in this embodiment are substantially the same as those in the aforementioned embodiment 1, except that the preparation steps are as follows:
[0060] Steps (1) and (2) are the same as in Example 1;
[0061] Step (3) Weigh 0.127 g of zirconium dinitrate hydrate, and immerse 2.0 g of the nanotube precursor in a mixed aqueous solution of nickel salt and zirconium dinitrate hydrate by an equal volume impregnation method to obtain a Ni / Ce 0.97 Zr 0.03 O2 catalyst, other aspects are the same as those of Comparative Example 1;
[0062] Step (4), the catalyst (Ni / Ce 0.97 Zr 0.03 O2) has a Ni loading of 4.73 wt%, and a molar ratio of x = 0.03 for Zr-doped Ce sites. Figure 2 The XRD analysis results show that, similar to Example 1, in the Ni / Ce 0.97 Zr 0.03 Zr in the O2 catalyst is also doped into the CeO2 lattice to form Ce 1-x Zr x O2 solid solution.
[0063] Step (5) using Ni / Ce 0.97 Zr 0.03 O2 catalyst replaced Ni / CeO2 catalyst, and the rest was the same as Comparative Example 1. The test results and TG-DTG analysis of the catalyst used are shown in the attached Figure 6 and Figure 4 From the attached Figure 6 It can be seen that Ni / Ce 0.97 Zr 0.03 O2 Catalysts X CO2 , X CH4 and R H2 / CO It decreases with the extension of reaction time but not as obvious as that of Ni / CeO2 catalyst, and the catalyst has a carbon deposition amount of 25.18% in the 10h performance test, indicating that when the molar ratio x of Zr doped Ce position is 0.03, the anti-carbon deposition performance of the catalyst is further improved.
[0064] Example 3
[0065] The carbon deposition resistant nickel-based catalyst, preparation method and application thereof for methane carbon dioxide dry reforming provided in this embodiment are substantially the same as those in the above-mentioned embodiments 1 and 2, except that the preparation steps are as follows:
[0066] Steps (1) and (2) are the same as in Example 1;
[0067] Step (3) Weigh 0.253 g of zirconium dinitrate hydrate, and immerse 2.0 g of the nanotube precursor in a mixed aqueous solution of nickel salt and zirconium dinitrate hydrate by an equal volume impregnation method to obtain a Ni / Ce 0.93 Zr 0.07O2 catalyst, other aspects are the same as those of Comparative Example 1;
[0068] Step (4), the catalyst (Ni / Ce 0.93 Zr 0.07 The loading amount of Ni in the catalyst was 3.70 wt % and the molar ratio of Zr to Ce was x=0.07. The morphology of the catalyst was analyzed by SEM and TEM. Figure 1 This is a scanning electron microscope (SEM)-transmission electron microscope (TEM) image of the catalyst prepared in Example 3 Comparative Example 1.
[0069] See attached Figure 1 After Zr was doped into the crystal structure of CeO2 nanotubes, the morphology of CeO2 nanotubes and the highly dispersed active metal nickel did not change significantly. Figure 2 The XRD analysis results show that, similar to Example 1, in the Ni / Ce 0.93 Zr 0.07 Zr in the O2 catalyst is also doped into the CeO2 lattice to form Ce 1-x Zr x O2 solid solution.
[0070] Step (5) using Ni / Ce 0.93 Zr 0.07 O2 catalyst replaced Ni / CeO2 catalyst, and the rest was the same as Comparative Example 1. The test results and TG-DTG analysis of the catalyst used are shown in the attached Figure 7 and Figure 4 From the attached Figure 4 and Figure 7 It can be seen that the catalyst has only 5.24% carbon deposition in the 10-hour performance test and the catalytic activity is highly maintained, indicating that Ni / Ce 0.93 Zr 0.07 O2 catalyst has better anti-carbon deposition performance than Ni / CeO2 catalyst.
[0071] Example 4
[0072] The anti-carbon deposition nickel-based catalyst, preparation method and application thereof for methane carbon dioxide dry reforming provided in this embodiment are substantially the same as those in the above-mentioned embodiments 1-3, except that the preparation steps are as follows:
[0073] Steps (1) and (2) are the same as in Example 1;
[0074] Step (3) Weigh 0.507 g of zirconium dinitrate hydrate, and immerse 2.0 g of the nanotube precursor in a mixed aqueous solution of nickel salt and zirconium dinitrate hydrate by an equal volume impregnation method to obtain a Ni / Ce 0.90 Zr 0.10O2 catalyst, other aspects are the same as those of Comparative Example 1;
[0075] Step (4), the catalyst (Ni / Ce 0.90 Zr 0.10 O2) has a Ni loading of 3.90 wt%, and a molar ratio of Zr doped Ce sites of x=0.10.
[0076] Step (5) using Ni / Ce 0.90 Zr 0.10 O2 catalyst replaced Ni / CeO2 catalyst, and the rest was the same as Comparative Example 1. The test results and TG-DTG analysis of the catalyst used are shown in the attached Figure 8 and Figure 4 From the attached Figure 4 and Figure 8 It can be seen that the catalyst has a carbon deposition rate of 39.06% in the 10h performance test, which is higher than that of Ni / Ce. 0.93 Zr 0.07 The O2 catalyst has a lower CO2 conversion rate and a higher carbon deposition amount, indicating that in the catalysts prepared in Comparative Example 1 and Examples 1-4, the Ni / Ce 0.93 Zr 0.07 O2 catalyst has the best anti-carbon deposition performance.
[0077] Example 5
[0078] The anti-carbon deposition nickel-based catalyst, preparation method and application thereof for methane carbon dioxide dry reforming provided in this embodiment are substantially the same as those in the above-mentioned embodiments 1-4, except that the preparation steps are as follows:
[0079] Steps (1) and (2) are the same as in Example 1;
[0080] Steps (3) and (4) are the same as in Example 3;
[0081] Step (5) using Ni / Ce 0.93 Zr 0.07 The catalytic performance data of the O2 catalyst for the dry reforming reaction of methane and carbon dioxide for 100 h were collected, and the rest was the same as in Example 3; the test results and the TG-DTG analysis of the catalyst used are respectively shown in the attached Fig. 9 and Figure 4 From the attached Figure 4 and Fig. 9It can be seen that in the methane carbon dioxide dry reforming reaction at 550°C, the carbon deposition of the catalyst in the 100h performance test was only 6.88%, which was not significantly increased compared to the 5.24% carbon deposition in the 10h test. Its catalytic activity was highly maintained, the carbon dioxide conversion rate was maintained at about 90%, and the methane conversion rate was maintained at more than 93%. The catalyst effectively solves the problems of high conversion temperature, easy carbon deposition and deactivation, and short service life of nickel-based catalysts in the methane carbon dioxide dry reforming reaction.
[0082] Comparative Example 1
[0083] A carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming, a preparation method and an application thereof, wherein the process steps are as follows:
[0084] (1) Preparation of Ce-MOF template:
[0085] The Ce-MOF template was prepared by a solvent method. Ce nitrate hexahydrate (4.34 g, 0.01 mol) and 1,3,5-benzenetricarboxylic acid (2.10 g, 0.01 mol) were dissolved in a mixed solution of anhydrous ethanol (10 mL) and deionized water (55 mL). The mixture was stirred at 70 ° C for 1 h to form a precipitate. The product was filtered after cooling to room temperature, washed alternately with deionized water and anhydrous ethanol three times, and dried in a forced air drying oven at 80 ° C overnight. The obtained white precipitate was the Ce-MOF template.
[0086] (2) Preparation of thin-walled CeO2 nanotube precursor:
[0087] The Ce-MOF template was heated to 600° C. in a muffle furnace at a rate of 10° C. / min and calcined for 3 h to obtain a thin-walled CeO2 nanotube precursor;
[0088] (3)Ni / Ce 1-x Zr x Synthesis of O2 catalyst:
[0089] Weigh 0.496g Ni(NO3)2·6H2O and 0g zirconium dinitrate hydrate, and use the equal volume impregnation method to immerse 2.0g of the nanotube precursor in a nickel salt aqueous solution, stand at room temperature for 2h, dry in a forced air drying oven to constant weight, and calcine it in a muffle furnace at 10℃ / min to 600℃ for 2h to obtain a calcined but unreduced Ni / CeO2 catalyst. Subsequently, the calcined sample is placed in a quartz fixed bed reactor equipped with a K-type thermocouple, with an inner diameter of 9mm and a length of 360mm, and reduced at 10℃ / min to 600℃ for 1h in a 20mL / min pure hydrogen atmosphere to obtain a Ni / CeO2 catalyst with highly dispersed nickel metal.
[0090] (4) Characterization and analysis of catalysts
[0091] The Ni loading in the catalyst (Ni / CeO2) was measured by ICP-OES to be 4.91 wt %, and the molar ratio of Zr doped Ce position was x=0. The morphology of the catalyst was analyzed by SEM and TEM, see Appendix Figure 1 The unclosed or defective structure indicates that the CeO2 derived from the Ce-MOF template is composed of thin-walled, hollow nanotubes, and the active metal nickel is evenly distributed on the surface of the CeO2 nanotubes. The crystal structure of the catalyst was analyzed by X-ray diffraction (XRD), see Appendix Figure 2 At 2θ=28.5°, 33.1°, 47.5°, 56.3°, 59.1°, 69.5°, 76.7° and 79.1°, characteristic diffraction peaks attributed to the (111), (200), (220), (311), (222), (400), (331) and (420) crystal planes of CeO2 can be clearly observed, but the characteristic diffraction peaks of active metal nickel are not obvious, indicating the successful preparation of Ce-MOF template-derived CeO2 and the high dispersion of active metal nickel.
[0092] (5) Testing the catalytic performance of the above catalyst:
[0093] After the catalyst was reduced in a quartz fixed bed reactor, high-purity nitrogen was introduced and the temperature was raised to 550°C at a rate of 10°C / min, and then a reaction gas mixture (CO2 / CH4 / N2 = 1 / 1 / 8, space velocity 3000 mL·h) with a total volume flow rate of 50 mL / min was introduced. -1 ·g cat -1 ) was reacted, and the tail gas was cooled in an ice-water bath and analyzed online using a FuLi9790 gas chromatograph (GC) equipped with both FID and TCD detectors to calculate and analyze the conversion rates of CO2 and CH4 (X CO2 and X CH4 ) and H2 / CO ratio (R H2 / CO ), collect the catalytic performance data of the reaction for 10 h, the test results and the TG-DTG analysis of the catalyst used are respectively shown in the attached Figure 3 and Figure 4 .
[0094] From the attached Figure 3 It can be seen that the X of the catalyst CO2 , X CH4 and R H2 / CO It decreases significantly with the extension of reaction time. In the early stage of the reaction, the H2 / CO ratio is greater than 1 due to the rapid cracking of CH4, but in the later stage of the reaction, due to the gradual deactivation of the catalyst and the occurrence of the reverse water gas side reaction, the H2 / CO ratio is significantly less than 1, indicating that the undoped Zr Ni / CeO2 catalyst is gradually deactivated. Figure 4It can be seen that during the test process of 10h of methane carbon dioxide dry reforming reaction at 550℃, the Ni / CeO2 catalyst produced 71.27% carbon deposits, indicating that the catalyst was deactivated due to severe carbon deposition.
[0095] According to the above embodiments of the present invention, the CeO2 nanotubes derived from metal organic framework materials (MOFs) have large cavities and thin-walled structures, which can evenly anchor the active metal Ni and easily dope Zr into its lattice to form a solid solution; compared with the Ni / CeO2 catalyst, an appropriate amount of Zr doping is beneficial to promote the activation of CO2 and inhibit the excessive cracking of CH4, thereby improving the anti-carbon deposition performance of the catalyst in the 550°C methane carbon dioxide dry reforming reaction. 0.93 Zr 0.07 O2 has excellent anti-carbon deposition performance. The amount of carbon deposition in the 100h performance test has no significant change compared with that in 10h, and the catalytic activity is highly maintained. This catalyst effectively solves the problems of high conversion temperature, carbon deposition deactivation and short service life of nickel-based catalysts in the methane carbon dioxide dry reforming reaction.
[0096] The above embodiments of the present invention focus on using thin-walled CeO2 nanotubes derived from cerium-based MOF as a template as a precursor, impregnating nickel salt and zirconium salt to synthesize Ni / Ce with cerium-zirconium solid solution as a carrier. 1-x Zr x O2 catalyst, by regulating the molar ratio x (0.01≤x≤0.2) of the Zr-doped Ce position of the catalyst, promotes the kinetic balance between carbon formation and carbon removal in the DRM process, thereby obtaining a catalyst with good catalytic DRM activity and excellent anti-carbon deposition performance, so as to effectively solve the problems of high conversion temperature, carbon deposition deactivation and short service life of nickel-based catalysts in the methane carbon dioxide dry reforming reaction.
[0097] The anti-carbon deposition nickel-based catalyst prepared by combining the improved formula and process in the above-mentioned embodiment of the present invention has excellent anti-carbon deposition performance. The amount of carbon deposition in the 100h test has no obvious change compared with that in the 10h test, and the catalytic activity is highly maintained, which effectively solves the problems of high conversion temperature and carbon deposition deactivation of nickel-based catalysts in the methane carbon dioxide dry reforming reaction.
[0098] It should be particularly noted that within the scope of the above-described invention, other solutions obtained by selecting other formulations and processes can all achieve the technical effects of the invention, so they are no longer listed one by one.
[0099] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0100] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming, characterized in that: The following steps are involved: (1) preparing a cerium-based MOF template; (2) calcining the cerium-based MOF template to obtain a thin-walled nanotube precursor; (3) Using a mixed aqueous solution of nickel salt and zirconium dinitrate hydrate as an impregnation solution, the nanotube precursor is sequentially subjected to impregnation, drying, calcination and reduction treatment to prepare a carbon deposition resistant nickel-based catalyst.
2. The method for preparing the anti-carbon deposition nickel-based catalyst for methane carbon dioxide dry reforming according to claim 1, characterized in that: In step (1), the preparation process of the cerium-based MOF template comprises the following steps: The cerium salt and 1,3,5-benzenetricarboxylic acid are dissolved in a mixed solution of anhydrous ethanol and deionized water to react, and after the reaction is completed, the cerium-based MOF template is obtained after separation, precipitation, washing and drying.
3. The method for preparing the anti-carbon deposition nickel-based catalyst for methane carbon dioxide dry reforming according to claim 1, characterized in that: The reaction is carried out at a temperature of 25-100° C., a reaction time of 0.5-6 h, a mass of 1,3,5-benzenetricarboxylic acid of 2.10 g, a molar ratio of 1,3,5-benzenetricarboxylic acid to the cerium salt of 0.5-3:1, a volume of deionized water of 55 mL, and a volume ratio of deionized water to anhydrous ethanol of 1:1-8:
1.
4. The method for preparing the anti-carbon deposition nickel-based catalyst for methane carbon dioxide dry reforming according to claim 1, characterized in that: In step (2), the calcination temperature is 25-900°C, the heating rate is 3-15°C / min, and the calcination time is 0.5-6h.
5. The method for preparing the anti-carbon deposition nickel-based catalyst for methane carbon dioxide dry reforming according to claim 1, characterized in that: In step (3), an equal volume impregnation method is used for impregnation treatment, and the mass percentage of elemental nickel in the obtained anti-carbon deposition nickel-based catalyst is 0.1%-20% of the nanotube precursor; The molar ratio of the element zirconium to the element cerium is x:(1-x), wherein x=0.01-0.
2.
6. The method for preparing the anti-carbon deposition nickel-based catalyst for methane carbon dioxide dry reforming according to claim 1, characterized in that: In step (3), the calcination temperature is 500-900° C. and the calcination time is 1-5 hours.
7. The method for preparing a carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming according to claim 1, characterized in that: In step (3), the reduction treatment is carried out in a hydrogen atmosphere, the reduction temperature is 500-900° C., the reduction time is 0.5-4 h, and the pure hydrogen flow rate is 10-40 mL / min.
8. A carbon deposition resistant nickel-based catalyst for methane carbon dioxide dry reforming, characterized in that: The catalyst is prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the carbon deposition resistant nickel-based catalyst according to claim 8 in a methane and carbon dioxide dry reforming reaction.
10. The use of the anti-carbon deposition nickel-based catalyst according to claim 9 in the methane carbon dioxide dry reforming reaction, characterized in that: During the application of the anti-carbon deposition nickel-based catalyst, the process conditions for methane dry reforming are: reaction temperature is 400-800°C, reaction pressure is atmospheric pressure, the volume ratio of reaction gas is CO2:CH4:N2=1:1:(1-10), and the catalyst dosage is 50-200mg.
Citation Information
Patent Citations
Nickel-based catalyst, preparation method of nickel-based catalyst, reduction state nickel-based catalyst and method for preparing synthesis gas through methane auto-thermal reforming
CN106311250A
Preparation method of Ni-Ce-based catalyst for methane and carbon dioxide dry reforming
CN116351430A
Nickel-doped catalyst as well as preparation method and application thereof
CN117619402A
Supported low-temperature methane dry reforming catalyst as well as preparation method and application thereof
CN117753429A
Cited By
Methane dry reforming catalyst as well as preparation method and application thereof
CN121669246A