Catalyst with stable alloy structure as well as preparation method and application of catalyst
By using a stable Ni-Fe alloy catalyst composed of composite support MOn-ZrO2 and metal Ni and Fe in the methane dry reforming reaction, the problem of carbon deposit and deactivation of the catalyst at high temperature is solved, the performance and life of the catalyst are improved, and the performance and life of the catalyst are achieved. It has the effect of resisting carbon deposits.
Patent Information
- Application Number
- CN202410949643.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-12-06
Smart Images

Figure CN119075992A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and in particular relates to a catalyst with a stable alloy structure and a preparation method and application thereof. Background Art
[0002] With the rapid development of industry, energy has become the material basis for the survival and development of human society. At present, the world's basic energy is still the three major fossil energy sources of coal, oil and natural gas. Their continuous consumption will produce a large amount of greenhouse gases, causing a series of problems such as global warming and glacier melting. Methane dry reforming reaction (DRM) can convert two greenhouse gases, CO2 and CH4, into synthesis gas (CO and H2), and the synthesis gas can be used as a raw material for Fischer-Tropsch synthesis for further synthesis of high value-added chemicals. Methane dry reforming can not only alleviate environmental problems but also effectively utilize greenhouse gases. It is a green, environmentally friendly and sustainable development approach with good application prospects.
[0003] DRM reaction has a complex reaction system. In addition to the main reaction In addition, it is usually accompanied by side reactions such as reverse water gas shift (CO2+H2→CO+H2O), CH4 cracking (CH4→C+2H2) and CO disproportionation (2CO→C+CO2). In addition, the DRM reaction is a highly endothermic reaction that requires high temperatures to drive the reaction, but at high temperatures, the catalyst is often deactivated due to carbon deposition produced by CH4 cracking and CO disproportionation. It is impossible to improve the carbon deposition of the DRM reaction by changing the thermodynamic conditions of the reaction. Therefore, it is crucial to design and prepare efficient catalysts that are resistant to carbon deposition.
[0004] Various catalysts have been studied for the DRM reaction. Among them, Ni-based catalysts have attracted the interest of many researchers because of their low price and catalytic performance comparable to that of precious metals. Studies have found that the development of Ni-based bimetallic alloy catalysts plays an important role in improving catalyst activity and inhibiting the formation and elimination of carbon deposition in the DRM reaction. By forming an alloy structure, the electronic structure and geometric structure of Ni particles can be changed to optimize the particle size, redox properties and other properties. Ni particles, as the active center of the catalyst, can improve the catalyst's ability to resist carbon deposition by forming Ni-Fe alloys. Compared with Ni, Fe has a higher affinity for oxygen. In the DRM reaction, Fe is more likely to adsorb CO2 than Ni, which can increase the surface oxygen content of the catalyst and promote the formation of intermediate products containing carbon and oxygen species during the reaction. To a certain extent, carbon removal is achieved and the catalyst's ability to resist carbon deposition is improved. However, the oxygen-affinity Fe species is easily over-oxidized by CO2, resulting in Fe dealloying. As the number of iron and oxygen species increases, they will cover the surface of the active metal or migrate into the carrier, resulting in a decrease in catalyst performance.
[0005] Therefore, how to retain the carbon removal ability of Ni-Fe alloy while constructing a stable Ni-Fe alloy structure by selecting a suitable carrier is the key to improving the service life and anti-carbon deposition performance of the catalyst. Summary of the invention
[0006] In view of the above problems and the current demand for DRM reaction catalysts, the present invention provides a method for preparing a stable Ni-Fe alloy catalyst, the purpose of which is to improve the methane dry reforming performance of the catalyst while enhancing the catalyst's anti-carbon deposition ability and service life.
[0007] The present invention adopts the following technical solution: A catalyst with a stable alloy structure, composed of a composite carrier MO n -ZrO2, metal Ni and metal Fe, the molecular formula of the alloy structure catalyst is Ni x Fe / yMO n -ZrO2, wherein M is a metal; x represents the mass ratio of nickel to iron; and y represents the molar ratio of M to Zr.
[0008] Furthermore, 1≤x≤10, preferably 2≤x≤5; 0.01≤y≤0.30, preferably 0.05≤y≤0.20.
[0009] Furthermore, the Ni loading in the catalyst is 5 wt%-15 wt%.
[0010] Furthermore, the M includes at least one of Ca, Y, Mg, Ce, La, and Sc.
[0011] A method for preparing a catalyst with a stable alloy structure comprises the following steps: The first step is to synthesize the carrier: dissolve a certain molar ratio of zirconium salt and M salt in deionized water, stir on a magnetic stirrer for 30 min to prepare a solution in which the metal ions are uniformly mixed; In the second step, a precipitant is added to the above solution, the pH is adjusted, and the precipitate is aged; then the solution is centrifuged and washed until neutral, and the washed sample is placed in an oven at 100-120°C and dried for 12-24 hours, and finally calcined to obtain MO n - ZrO2 carrier; The third step is to synthesize the nickel-iron alloy catalyst: dissolve the nickel salt and iron salt in deionized water in proportion to form a uniform solution, and then n -ZrO2 carrier is added to the solution, stirred in a 50℃ water bath for 12-24h, then rotary evaporated, dried and calcined to obtain a fresh catalyst; In the fourth step, the fresh catalyst in the third step is reduced in a hydrogen environment for 1-2 hours to obtain the target catalyst Ni x Fe / yMOn -ZrO2.
[0012] Furthermore, in the first step, the zirconium salt includes any one of zirconium nitrate, zirconium oxychloride, and zirconium chloride, or a mixture of several thereof; the M salt includes one of nitrate, sulfate, and acetate; and the molar ratio of the M salt to the zirconium salt is 0.05-0.20.
[0013] Furthermore, in the first step, the concentration of the zirconium salt in the solution is 0.1-1 mol / L, preferably 0.5-1 mol / L; the concentration of the M salt in the solution is 0.1-1 mol / L, preferably 0.5-1 mol / L.
[0014] Furthermore, in the second step, the precipitant comprises any one or a mixture of urea, ammonia water, sodium hydroxide, sodium carbonate, potassium hydroxide, and the concentration of the precipitant is 0.1-0.5 mol / L, preferably 0.3-0.5 mol / L; the pH of the solution is adjusted to 9-12, preferably 10-11.
[0015] Furthermore, in the second step, the aging precipitation time is 12-24 hours, preferably 18-24 hours; the calcination temperature is 400-600° C., preferably 500-600° C., and the calcination time is 2-4 hours, preferably 2-3 hours.
[0016] Furthermore, in the third step, the nickel salt includes one or a mixture of nickel nitrate, nickel sulfate, and nickel acetate, and the iron salt includes one or a mixture of iron nitrate, iron sulfate, and iron acetate; the mass ratio of nickel to iron is 2-5; the concentration of the nickel salt in the solution is 0.5-2 mol / L; preferably 1-2 mol / L, and the concentration of the iron salt in the solution is 0.5-2 mol / L, preferably 1-2 mol / L.
[0017] Furthermore, in the third step, the rotary evaporation temperature is 40-60°C, the roasting temperature is 400-600°C, preferably 500-600°C, and the roasting time is 3-6h, preferably 4-5h.
[0018] Furthermore, in the fourth step, the hydrogen flow rate is 10-30 mL / min, and the reduction temperature is 600-800°C.
[0019] A catalyst with a stable alloy structure is applied to methane dry reforming reaction.
[0020] The principle of the present invention is as follows: Through this method, a methane dry reforming catalyst with a stable nickel-iron alloy structure can be synthesized, especially by doping with M ions, a zirconium oxide carrier with a stable tetragonal phase crystal form is synthesized, and this carrier will not undergo a crystal form change under a high temperature environment, and can better stabilize the nickel-iron alloy. The catalyst has excellent methane dry reforming performance, and the stable nickel-iron alloy structure improves the catalyst's anti-carbon deposition ability and service life.
[0021] The beneficial effects of the present invention are as follows: Being able to synthesize a catalyst with a stable Ni-Fe alloy structure not only improves the catalytic performance of the catalyst, but also greatly improves the catalyst's resistance to carbon deposition and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the XRD pattern of the carrier in experimental group 2.
[0023] Figure 2 This is the BET diagram of the carrier in experimental group 2.
[0024] Figure 3 This is the SEM image of the carrier in experimental group 2.
[0025] Figure 4 This is the XRD pattern of the fresh catalyst in experimental group 3.
[0026] Figure 5 This is the BET diagram of the fresh catalyst in experimental group 3.
[0027] Figure 6 This is the SEM image of the fresh catalyst in experimental group 3.
[0028] Figure 7 This is the XRD pattern of the reduced catalyst in Experimental Group 4.
[0029] Figure 8 This is the catalyst activity test diagram in test group 1.
[0030] Fig. 9 This is the catalyst stability test chart in test group 3.
[0031] Fig.10 This is the XRD diagram of the catalyst in test group 3 after stability test.
[0032] Fig.11 This is the SEM image of the catalyst in test group 3 after stability test. DETAILED DESCRIPTION
[0033] The following embodiments are not intended to limit the present invention in any way. For those skilled in the art, the present invention may have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0034] Embodiment 1 A method for preparing a catalyst having a stable alloy structure comprises: Step S1: dissolving M salt (M is one of Ca, Y, Mg, Ce, La, and Sc) and zirconium salt in a molar ratio of 0.05-0.20 in 100 mL of deionized water to prepare solution A, and stirring solution A on a magnetic stirrer for 30 min to allow the metal ions to be completely mixed; Step S2: adding a precipitant selected from urea, ammonia water, sodium hydroxide, sodium carbonate and potassium hydroxide to solution A, adjusting the pH of the solution to 10-11, and aging and precipitating for 18-24 h; then centrifugally washing with deionized water and ethanol until neutral, placing the washed product in an oven at 100-120° C. and drying it for 12-24 h to obtain a white solid product, grinding the white product into powder, and finally roasting it at 500-600° C. for 2-3 h to obtain an oxide carrier B; Step S3: first, the nickel loading is fixed to 5 wt%-15 wt%, then nickel salt and iron salt with a mass ratio of 2-5 are dissolved in 20 mL of deionized water to prepare a uniform solution C, the carrier B is added to the solution C, and stirred in a 50 ° C water bath for 12-24 h, and finally the mixed solution C is rotary evaporated at 40-60 ° C, dried, and calcined at 500-600 ° C for 4-5 h to obtain a fresh catalyst D; Step S4: The fresh catalyst D obtained by calcination is reduced in a hydrogen atmosphere for 1-2 h to obtain the target catalyst Ni x Fe / yMO n -ZrO2, the hydrogen flow rate is 10-30 mL / min, and the reduction temperature is 600-800 ℃.
[0035] Through this method, a methane dry reforming catalyst with a stable nickel-iron alloy structure can be synthesized, especially by doping with M ions, a zirconium oxide carrier with a stable tetragonal phase crystal form is synthesized, and this carrier will not undergo a crystal form change under a high temperature environment, and can better stabilize the nickel-iron alloy. The catalyst has excellent methane dry reforming performance, and the stable nickel-iron alloy structure improves the catalyst's anti-carbon deposition ability and service life.
[0036] In step S1, the molar ratio of zirconium salt to M salt is preferably 5%, 10%, 15%, 20%. The zirconium salt used is one of zirconium nitrate, zirconium oxychloride, and zirconium chloride, and the concentration of the zirconium salt solution is preferably 0.5-1 mol / L. The M salt used is one of nitrate, sulfate, and acetate, and the concentration of the M salt solution is preferably 0.5-1 mol / L. In step S2, the concentration of the precipitant is preferably 0.3-0.5 mol / L, and the pH of the solution is adjusted to 10 and 11, respectively. The aging precipitation time is preferably 18 h, 20 h, 22 h, 24 h. The roasting temperature is preferably 500 °C, 550 °C, 600 °C. The roasting time is preferably 2 h and 3 h.
[0037] In step S3, the nickel loading is 5 wt%, 10 wt%, 15 wt%, and the mass ratio of nickel to iron is preferably 2, 3, 4, 5. The nickel salt is one of nickel nitrate, nickel sulfate, and nickel acetate, and the concentration of the nickel salt solution is preferably 1-2 mol / L. The iron salt is one of iron nitrate, iron sulfate, and iron acetate, and the concentration of the iron salt solution is preferably 1-2 mol / L. In step S3, the rotary evaporation temperature is preferably 60°C, the calcination temperature is preferably 500°C, 550°C, 600°C, and the calcination time is preferably 4 h and 5 h.
[0038] In step S4, the hydrogen flow rate is preferably 30 mL / min, the reduction temperature is preferably 600°C, 700°C, 800°C, and the reduction time is preferably 1 h and 2 h.
[0039] Embodiment 2 A catalyst with a stable alloy structure can be prepared by the method provided in Example 1. The molecular formula of the catalyst is Ni x Fe / yMO n -ZrO2, where x represents the mass ratio of nickel to iron, and y represents the molar ratio of M to Zr.
[0040] Preferably, 2≤x≤5.
[0041] Preferably, 0.05≤y≤0.20.
[0042] Preferably, the nickel loading in the catalyst is 5 wt%.
[0043] In some specific embodiments, the molecular formula of the supported nickel-based catalyst is Ni3Fe / 15CaO-ZrO2.
[0044] Embodiment 3 An application of a catalyst with a stable alloy structure is to apply the supported alloy catalyst prepared in Example 2 to a methane dry reforming reaction.
[0045] Embodiment 4 A method for converting greenhouse gas into synthesis gas comprises contacting carbon dioxide and methane with the supported nickel-iron alloy catalyst of Example 2 under methane dry reforming reaction conditions.
[0046] Preferably, the above contact reaction is carried out in a micro fixed bed reactor, and the reaction conditions are that the ratio between methane and carbon dioxide is 1:1, the total flow rate is 50 mL / min, the reaction temperature is 650-800 ° C, and the reaction pressure is normal pressure, where normal pressure refers to one atmosphere, i.e. 1 bar.
[0047] Some specific experimental groups and test / characterization results are provided below Experimental Group 1 Weigh 3.222 g of zirconium oxychloride octahydrate (ZrOCl2·8H2O) and 0.417 g of calcium nitrate tetrahydrate (Ca(NO3)2·4H2O) (the molar ratio of calcium salt to zirconium salt is 15%), dissolve them in 100 mL of deionized water, and stir the prepared solution on a magnetic stirrer for 30 min to mix the metal ions evenly.
[0048] Experimental Group 2 0.1 mol / mL of ammonia water was slowly dripped into the prepared solution to adjust the pH value to 10, and the precipitate was aged for 24 hours, and then centrifuged and washed with water and alcohol until the solution was neutral. The obtained product was placed in a 100 ℃ oven and dried for 12 hours, and ground to obtain a white powder. Finally, the white powder was ground and calcined in a 600 ℃ muffle furnace for 3 hours to obtain the target carrier.
[0049] Experimental Group 3 Weigh 0.531 g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O) and 0.258 g of ferric nitrate nonahydrate (Fe(NO3)3·9H2O) in a round-bottom flask (the nickel loading is 5 wt%, and the mass ratio of nickel to iron is 3), add 20 mL of deionized water to fully dissolve, then add 2.000 g of the carrier powder prepared in experimental group 2, and then stir in a 50°C water bath for 12 h. The stirred solution was rotary evaporated at 60°C until the solvent was completely evaporated, and the obtained sample was further dried. Finally, it was calcined in a muffle furnace at 500°C for 4 h to obtain a fresh catalyst.
[0050] Experimental Group 4 The calcined fresh catalyst obtained in Experimental Group 3 was reduced in a hydrogen (30 mL / min) atmosphere for 1 h to obtain the target catalyst Ni3Fe / 15CaO-ZrO2 at a reduction temperature of 700 °C.
[0051] Experimental Groups 5-7 The difference between experimental groups 5-7 and experimental group 1 is that the molar ratio of the added calcium salt to the zirconium salt is 5%, 10%, and 20%, and the other steps are the same.
[0052] Experimental Group 8-9 The difference between experimental groups 8-9 and experimental group 1 is that the added M salts are yttrium nitrate hexahydrate (Y(NO3)3·6H2O) and magnesium nitrate hexahydrate (Mg(NO3)2·6H2O), and the other steps are the same.
[0053] The following tests / characterizations are performed for the above experimental groups 1. White solid powder obtained from experimental group 2 Figure 1 is the XRD pattern of 15CaO-ZrO2 carrier in experimental group 2. Figure 1 It can be seen that 15CaO-ZrO2 has typical characteristic diffraction peaks belonging to tetragonal zirconia at 30.34±0.1°, 35.16±0.1°, 50.54±0.1°, 60.10±0.1°, 62.57±0.1° and 73.83±0.1°. The incorporation of calcium ions stabilizes zirconia into a tetragonal phase. No characteristic diffraction peaks belonging to calcium oxide were observed. This is because when the calcium content is low, Ca 2+ Inserted into the ZrO2 lattice to form a uniform CaO-ZrO2 solid solution.
[0054] Figure 2 This is the SEM image of the carrier in experimental group 2, which shows the morphological characteristics of the 15CaO-ZrO2 carrier.
[0055] Figure 3 (a) N2 adsorption-desorption diagram and (b) pore size distribution diagram of the carrier in Experimental Group 2. Figure 3 It can be seen that the adsorption-desorption isotherm of 15CaO-ZrO2 conforms to the classic type IV isotherm and has an H3 type hysteresis loop, indicating the existence of a mesoporous structure.
[0056] The specific surface area, average pore size and pore volume of the carrier 15CaO-ZrO2 in experimental group 2 are shown in Table 1.
[0057] Table 1 Specific surface area, average pore size, and pore volume of carrier 15CaO-ZrO2 in experimental group 2 2. Fresh catalyst obtained from experimental group 3 Figure 4 This is the XRD pattern of the fresh catalyst in Experimental Group 3. The fresh catalyst after calcination showed characteristic diffraction peaks belonging to nickel oxide and iron oxide species. Due to the small amount of metal loading and high dispersion, the peak intensity of nickel oxide and iron oxide species is weak. The structure of the carrier did not change significantly after calcination and still maintained the tetragonal phase.
[0058] Figure 5 (a) N2 adsorption-desorption diagram and (b) pore size distribution diagram of fresh catalyst in Experimental Group 3. Figure 5 It can be seen that the adsorption-desorption isotherm of the calcined catalyst is still a type IV isotherm with an H3 type hysteresis loop and a mesoporous structure.
[0059] Table 2 shows the specific surface area, average pore diameter and pore volume of the fresh catalyst in experimental group 3.
[0060] Table 2 Specific surface area, average pore diameter, and pore volume of fresh catalyst in experimental group 3 Figure 6 This is the SEM image of the fresh catalyst in Experimental Group 3. This shows the morphological characteristics of the fresh catalyst.
[0061] 3. The reduced catalyst obtained from experimental group 4 Figure 7 is the XRD pattern of the catalyst after reduction in Experimental Group 4. Figure 7 It can be seen that the reduced catalyst has a characteristic diffraction peak belonging to Ni3Fe at 44.2°±0.1°, indicating that the reduced catalyst forms a Ni3Fe alloy structure.
[0062] The methane dry reforming performance of the catalysts prepared in experimental groups 4-9 was evaluated.
[0063] Test Group 1 The methane dry reforming activity of the catalyst prepared in Experimental Group 4 was tested using a micro fixed bed reactor. The quartz tube used had an outer diameter of 12 mm, an inner diameter of 8 mm, and a length of 485 mm.
[0064] Mix 0.1 g catalyst (20-40 mesh) and 1 g quartz sand (20-40 mesh) evenly and load into the constant temperature zone of the fixed bed reactor to check the air tightness of the device. After purging with Ar (30 mL / min) for 10 min, heat to 700 °C and switch to H2 (30 mL / min) to reduce the catalyst for 1 h. Then switch the feed gas to a mixture of CH4 and CO2 (CH4 / CO2=1 / 1, total flow rate of 50 mL / min) to test the methane dry reforming activity of the catalyst.
[0065] The reaction products were analyzed by online gas chromatography equipped with a thermal conductivity detector (TCD), and the tail gas velocity was measured by a soap bubble flowmeter. The test temperature range was 700-800°C, the temperature increase gradient was 50°C, and the test time at each temperature point was 1 h.
[0066] Test Group 2 The catalysts prepared in Experimental Groups 5 to 9 were tested for methane dry reforming activity under the same test conditions as those in Experimental Group 1.
[0067] Test Group 3 The catalyst prepared in Experimental Group 4 was subjected to a methane dry reforming stability test, and the stability test was also carried out on a micro fixed bed reactor.
[0068] 0.1 g of catalyst (20-40 mesh) and 1 g of quartz sand (20-40 mesh) were mixed evenly and loaded into the constant temperature zone of the fixed bed reactor to check the air tightness of the device. After purging with Ar (30 mL / min) for 10 min, the temperature was raised to 700°C and switched to H2 (30 mL / min) to reduce the catalyst for 1 h. Then, the temperature was raised to 800°C under Ar (30 mL / min) atmosphere, and the raw gas was switched to a mixture of CH4 and CO2 (CH4 / CO2=1 / 1, total flow rate of 50 mL / min) to test the catalyst for methane dry reforming stability.
[0069] The reaction products were analyzed by online gas chromatography equipped with a thermal conductivity detector (TCD), and the tail gas velocity was measured by a soap bubble flow meter. The test time was 10 h.
[0070] Test Group 4 The catalysts prepared in test groups 5-9 were subjected to a methane dry reforming stability test, and the test conditions were the same as those of test group 3.
[0071] Figure 8 This is the activity test diagram of the catalyst in test group 1. Figure 8 It can be seen that within 700-800°C, the CH4 conversion rate of the Ni3Fe / 15CaO-ZrO2 catalyst increases from 62% to 83%, the CO2 conversion rate increases from 78% to 93%, and the H2 / CO ratio increases from 0.93 to 0.98. The Ni3Fe / 15CaO-ZrO2 catalyst prepared by the present invention has good methane dry reforming performance.
[0072] Table 3 is obtained based on the test data of test group 2: Table 3 Methane dry reforming activity test of different catalysts Fig. 9This is the stability test diagram of the catalyst in test group 3. Fig. 9 It can be seen that the Ni3Fe / 15CaO-ZrO2 catalyst has good methane dry reforming stability.
[0073] Table 4 is obtained based on the test data of test group 4: Table 4 Stability test of methane dry reforming of different catalysts Fig.10 The XRD diagram of the catalyst after the stability test in test group 3. Fig.10 It can be seen that the catalyst still has a Ni-Fe alloy structure after the stability test, and the carrier after the reaction is still a tetragonal crystal, indicating that the tetragonal zirconia carrier can stabilize the nickel-iron alloy well.
[0074] Fig.11 This is the SEM image of the catalyst stability test in test group 3. Fig.11 It can be seen that no obvious carbon deposits are produced on the catalyst after the reaction.
[0075] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations that fall within the meaning and scope of the equivalent elements of the claims be included in the invention.
[0076] In addition, it should be understood that although the present specification is described in accordance with implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
Claims
1. A catalyst having a stable alloy structure, characterized in that: The catalyst is composed of a composite carrier MO n -ZrO2, metal Ni and metal Fe, the molecular formula of the alloy structure catalyst is Ni x Fe / yMO n -ZrO2, wherein M is a metal; x represents the mass ratio of nickel to iron; and y represents the molar ratio of M to Zr.
2. The catalyst having a stable alloy structure according to claim 1, characterized in that: Said 1≤x≤10; 0.01≤y≤0.
30.
3. The catalyst having a stable alloy structure according to claim 1, characterized in that: The Ni loading amount in the catalyst is 5 wt%-15 wt%.
4. The catalyst having a stable alloy structure according to claim 1, characterized in that: The M includes at least one of Ca, Y, Mg, Ce, La, and Sc.
5. A method for preparing a catalyst having a stable alloy structure as claimed in claim 1, characterized in that: The steps include: The first step is to synthesize the carrier: dissolve a certain molar ratio of zirconium salt and M salt in deionized water, stir on a magnetic stirrer for 30 minutes to prepare a solution in which the metal ions are uniformly mixed; In the second step, a precipitant is added to the above solution, the pH is adjusted, and the precipitate is aged; then the solution is centrifuged and washed until neutral, and the washed sample is placed in an oven at 100-120°C and dried for 12-24 h, and finally calcined to obtain MO n - ZrO2 carrier; The third step is to synthesize the nickel-iron alloy catalyst: dissolve the nickel salt and iron salt in deionized water in proportion to form a uniform solution, and then n -ZrO2 carrier is added to the solution, stirred in a 50℃ water bath for 12-24h, then rotary evaporated, dried and calcined to obtain a fresh catalyst; In the fourth step, the fresh catalyst described in the third step is reduced in a hydrogen environment for 1-2 hours to obtain the target catalyst Ni x Fe / yMO n -ZrO2.
6. The method for preparing a catalyst having a stable alloy structure according to claim 5, characterized in that: In the first step, the zirconium salt includes any one of zirconium nitrate, zirconium oxychloride, and zirconium chloride, or a mixture thereof; the M salt includes one of nitrate, sulfate, and acetate; and the molar ratio of the M salt to the zirconium salt is 0.05-0.20; In the first step, the concentration of zirconium salt in the solution is 0.1-1 mol / L; the concentration of M salt in the solution is 0.1-1 mol / L.
7. The method for preparing a catalyst having a stable alloy structure according to claim 5, characterized in that: In the second step, the precipitant includes any one or a mixture of urea, ammonia water, sodium hydroxide, sodium carbonate, potassium hydroxide, the concentration of the precipitant is 0.1-0.5 mol / L, and the pH of the solution is adjusted to 9-12; The aging precipitation time in the second step is 12-24 hours; the roasting temperature is 400-600° C., and the roasting time is 2-4 hours.
8. The method for preparing a catalyst having a stable alloy structure according to claim 5, characterized in that: In the third step, the nickel salt includes one or a mixture of nickel nitrate, nickel sulfate, and nickel acetate, and the iron salt includes one or a mixture of iron nitrate, iron sulfate, and iron acetate; the mass ratio of nickel to iron is 2-5; the concentration of the nickel salt in the solution is 0.5-2 mol / L; the concentration of the iron salt in the solution is 0.5-2 mol / L; In the third step, the rotary evaporation temperature is 40-60° C., the roasting temperature is 400-600° C., and the roasting time is 3-6 hours.
9. The method for preparing a catalyst having a stable alloy structure according to claim 5, characterized in that: In the fourth step, the hydrogen flow rate is 10-30 mL / min, and the reduction temperature is 600-800°C.
10. A catalyst with a stable alloy structure as claimed in claim 1 used in a methane dry reforming reaction.
Citation Information
Patent Citations
Nickel-based catalyst, preparation method of nickel-based catalyst, reduction state nickel-based catalyst and method for preparing synthesis gas through methane auto-thermal reforming
CN106311250A
Preparation method and application of iron-doped lanthanum oxide-supported nickel-based catalyst
CN109046364A
Catalyst for preparing hydrogen through catalytic cracking of methanol and preparation method of catalyst
CN109999813A
Catalyst for conversion reaction of C2 < + > alkane and carbon dioxide to synthesis gas and preparation
CN115888725A