Carbon-coated cerium phosphate composite material as well as preparation method and application thereof

By forming a carbon layer on the surface of cerium phosphate nanoparticles, the problem of low efficiency of cerium phosphate photocatalysts is solved, and a carbon-coated cerium phosphate composite material with high efficiency photocatalytic performance is achieved, which simplifies the preparation process and improves stability and photocatalytic effects.

CN118904368AInactive Publication Date: 2024-11-08HUNAN UNIV OF HUMANITIES SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410951738.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing cerium phosphate photocatalysts are inefficient in photocatalytic applications, mainly due to the high probability of photogenerated electron-hole recombination, resulting in poor photocatalytic effect.

Method used

Carbon-coated cerium phosphate composite material is used to form a carbon layer coated cerium phosphate nanoparticles in hydrothermal reaction through phytic acid as a reducing agent to improve photocatalytic performance.

Benefits of technology

It improves the stability and photocatalytic efficiency of the material, enhances the separation ability of photogenerated electrons and holes, achieves high-performance photocatalytic effects, and simplifies the preparation process to facilitate large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904368A_ABST
    Figure CN118904368A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon-coated cerous phosphate composite material and a preparation method and application thereof, and belongs to the technical field of catalytic material preparation, and the carbon-coated cerous phosphate composite material is prepared from the following raw materials in parts by weight: 1-3 parts of Ce (SO4) 2, 5-20 parts of pure water, 2-5 parts of 98% sulfuric acid and 0.5-3 parts of 70% phytic acid solution. According to the prepared carbon-coated cerous phosphate composite material, the stability of the material is improved through introduction of a carbon layer, meanwhile, separation of photo-induced electrons and holes in cerous phosphate is promoted through the electron transmission characteristic of carbon, and the photocatalytic efficiency of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic material preparation, and specifically relates to a carbon-coated cerium phosphate composite material and a preparation method and application thereof. Background Art

[0002] Water pollution control and water environment protection are important research areas for sustainable development of the ecological environment. Research on high-tech water treatment is not only the current research frontier in the field of international water science and technology, but also the need to solve water environmental pollution problems. Among the various environmental pollution treatment technologies, semiconductor photocatalysis technology is an effective method to use renewable energy to control water pollution and air pollution. Semiconductor photocatalysts are based on semiconductor materials. When the light energy is greater than the semiconductor bandgap, the electrons in the valence band (VB) are excited and jump to the conduction band (CB), generating photogenerated electrons (e - ) and holes (h + ), the photogenerated electrons and holes will react with the surrounding oxygen, water, etc. to generate highly active superoxide radicals and hydroxyl radicals, and the free radicals can effectively decompose pollutants in water. Hexagonal cerium phosphate is a type of photocatalytic material with great development potential and broad application prospects due to its narrow band gap (2.93eV) and ability to absorb visible light. However, the existing cerium phosphate generally exhibits low photocatalytic efficiency in photocatalytic applications, which is mainly because the probability of photogenerated electron-hole recombination in cerium phosphate is still very high, resulting in a low photocatalytic effect.

[0003] Carbon has a high specific surface area and good electrical conductivity. In the field of photocatalysis, carbon can effectively promote the transmission of photogenerated electrons and reduce the recombination of photogenerated electrons and holes. In particular, the formation of a carbon-coated semiconductor nanoparticle structure can significantly improve the separation of photogenerated electron-hole pairs and enhance the photocatalytic effect. However, the preparation of carbon-coated photocatalysts currently usually requires two steps. The first step is to wrap organic matter on the surface of the photocatalyst particles, and the second step is to pyrolyze the coating material at high temperature to form a carbon shell. Traditional carbon coating methods are complex and costly. Therefore, the development of a simple and efficient carbon-coated cerium phosphate composite material that obtains efficient photocatalytic performance is of great significance in the field of photocatalysis. Summary of the invention

[0004] The purpose of the present invention is to provide a carbon-coated cerium phosphate composite material and a preparation method and application thereof. The composite material has visible light response capability, can provide abundant active reaction points, and effectively realize the transmission of photogenerated electrons, and is a high-performance photocatalytic material.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0006] A carbon-coated cerium phosphate composite material comprises the following raw materials in parts by weight: 1-3 parts of Ce(SO4 ) 2 , 5-20 parts of pure water, 2-5 parts of 98% sulfuric acid, 0.5-3 parts of 70% phytic acid solution,

[0007] Preferably, the raw materials include the following parts by weight: 2 parts Ce(SO 4 ) 2 , 20 parts pure water, 3 parts sulfuric acid, 1.35 parts 70% phytic acid solution.

[0008] The present invention also provides a method for preparing a carbon-coated cerium phosphate composite material, comprising the following steps:

[0009] S1. Place Ce(SO 4 ) 2 Place in a beaker, add pure water and sulfuric acid to dissolve, stir evenly to obtain a mixed solution A;

[0010] S2, mixing 70% phytic acid solution with pure water to obtain a mixed solution B;

[0011] S3, mixing solution A and solution B, stirring evenly, adjusting the pH value of the solution with 20% NaOH solution, and then transferring the mixed solution to a reactor for hydrothermal reaction;

[0012] S4. Centrifuge or filter the mixture after the reaction, wash, dry and grind the obtained solid to obtain a composite material of carbon-coated cerium phosphate.

[0013] Preferably, in step S3, the pH value of the solution is adjusted to 2-11 using 20% ​​NaOH solution.

[0014] Further preferably, in step S3, the pH value of the solution is adjusted to 2 using 20% ​​NaOH solution.

[0015] Preferably, in step S3, the mixed solution is transferred to a reaction kettle and subjected to a hydrothermal reaction at 70-180° C. for 6-12 h.

[0016] Further preferably, in step S3, the mixed solution is transferred to a reactor and subjected to a hydrothermal reaction at 100° C. for 8 hours.

[0017] Preferably, in step S4, the obtained solid is washed and then dried at 60-120° C. for 30-120 min.

[0018] More preferably, in step S4, the obtained solid is washed and then dried at 80° C. for 60 min.

[0019] The present invention also provides application of the carbon-coated cerium phosphate composite material or the carbon-coated cerium phosphate composite material prepared by the preparation method as a photocatalytic material.

[0020] The technical scheme of the present invention is as follows: using phytic acid as a reducing agent, Ce(SO 4 ) 2 Ce 4+ Restore to Ce 3+ , and then combines with the phosphate in phytic acid to form cerium phosphate nanoparticles. At the same time, the excess phytic acid slowly forms carbon during the hydrothermal reaction and is evenly coated on the surface of the cerium phosphate nanoparticles to form a carbon-coated cerium phosphate composite material.

[0021] Compared with the prior art, the present invention has the following advantages and technical effects:

[0022] 1. The carbon-coated cerium phosphate composite material prepared by the present invention improves the stability of the material by introducing a carbon layer, and at the same time utilizes the electron transport properties of carbon to promote the separation of photogenerated electrons and holes in cerium phosphate, thereby improving the photocatalytic efficiency of the material.

[0023] 2. The carbon-coated cerium phosphate composite material of the present invention has excellent visible light response capability and effectively realizes the transmission of photogenerated electrons, and is a high-performance photocatalytic material.

[0024] 3. The method for preparing the carbon-coated cerium phosphate composite material of the present invention is simple to operate, efficient, convenient for large-scale production and industrial application, and can be extended to the preparation of other carbon-coated phosphate composite materials.

[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a transmission electron microscope image of the carbon-coated cerium phosphate composite material provided in Example 1;

[0027] Figure 2 is the X-ray diffraction pattern of Example 2;

[0028] Figure 3 The carbon-coated cerium phosphate composite material provided in Examples 1-3 and the Ce(SO 4 ) 2 Line graph of the material's degradation of methyl orange under visible light. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0030] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0031] Unless otherwise specified, the "parts" described in the present invention are all based on mass parts.

[0032] Source of experimental materials used in this invention: Ce(SO 4 ) 2 and 70% phytic acid solution were purchased from Aladdin Reagent Co., Ltd., and 98% sulfuric acid and sodium hydroxide powder were purchased from Hunan Huihong Reagent Co., Ltd.

[0033] Example 1 This example provides a carbon-coated cerium phosphate composite material

[0034] S1, 2 parts of Ce(SO 4 ) 2 Place in a beaker, add 10 parts of pure water and 3 parts of 98% sulfuric acid to dissolve, stir evenly to obtain a mixed solution A;

[0035] S2, mixing 1.35 parts of 70% phytic acid solution with 10 parts of pure water to obtain a mixed solution B;

[0036] S3, mixing solution A and solution B, stirring evenly, adjusting the pH value of the solution to 2 using 20% ​​NaOH by mass fraction, and then transferring the mixed solution to a reactor, and performing a hydrothermal reaction at 100° C. for 8 hours;

[0037] S4. The mixture after the reaction was filtered and washed with deionized water until the filtrate was neutral, and the obtained solid was dried in an oven at 80° C. for 60 min to obtain a composite material of carbon-coated cerium phosphate.

[0038] Example 2

[0039] S1, 2 parts of Ce(SO 4 ) 2 Place in a beaker, add 10 parts of pure water and 3 parts of 98% sulfuric acid to dissolve, stir evenly to obtain a mixed solution A;

[0040] S2, mixing 1.35 parts of 70% phytic acid solution with 10 parts of pure water to obtain a mixed solution B;

[0041] S3, mixing solution A and solution B, stirring evenly, adjusting the pH value of the solution to 2 using a 20% by mass NaOH solution, and then transferring the mixed solution to a reactor, and performing a hydrothermal reaction at 70° C. for 8 hours;

[0042] S4. The mixture after the reaction was filtered and washed with deionized water until the filtrate was neutral, and the obtained solid was dried in an oven at 80° C. for 60 min to obtain a composite material of carbon-coated cerium phosphate.

[0043] Example 3

[0044] S1, 2 parts of Ce(SO 4 ) 2 Place in a beaker, add 10 parts of pure water and 3 parts of 98% sulfuric acid to dissolve, stir evenly to obtain a mixed solution A;

[0045] S2, mixing 1.35 parts of 70% phytic acid solution with 10 parts of pure water to obtain a mixed solution B;

[0046] S3, solution A and solution B were mixed and stirred evenly, the pH value of the solution was adjusted to 2 with a 20% by mass NaOH solution, and the mixed solution was transferred to a reactor for hydrothermal reaction at 130° C. for 8 h;

[0047] S4. The mixture after the reaction was filtered and washed with deionized water until the filtrate was neutral, and the obtained solid was dried in an oven at 80° C. for 60 min to obtain a composite material of carbon-coated cerium phosphate.

[0048] Example 4

[0049] S1, 2 parts of Ce(SO 4 ) 2 Place in a beaker, add 10 parts of pure water and 3 parts of 98% sulfuric acid to dissolve, stir evenly to obtain a mixed solution A;

[0050] S2, mixing 1.35 parts of 70% phytic acid solution with 10 parts of pure water to obtain a mixed solution B;

[0051] S3, mixing solution A and solution B, stirring evenly, adjusting the pH value of the solution to 8 with a 20% by mass NaOH solution, and then transferring the mixed solution to a reactor, performing a hydrothermal reaction at 100° C. for 8 hours;

[0052] S4. The mixture after the reaction was filtered and washed with deionized water until the filtrate was neutral, and the obtained solid was dried in an oven at 80° C. for 60 min to obtain a composite material of carbon-coated cerium phosphate.

[0053] Comparative Example 1 provides a Ce(SO 4 ) 2 Material.

[0054] S1, 3.17 parts of Ce(CH 3 COO 3Place in a beaker, add 20 parts of pure water and 0.98 parts of 98% sulfuric acid to dissolve, stir evenly to obtain a mixed solution A;

[0055] S2, mixing 1.19 parts of sodium dihydrogen phosphate with 20 parts of pure water to obtain a mixed solution B;

[0056] S3, mixing solution A and solution B, stirring thoroughly, adjusting the pH value of the solution to 2 with a 20% by mass NaOH solution, and stirring the mixture in a 100° C. water bath for 8 h;

[0057] S4, the reaction mixture was filtered and washed with deionized water until the filtrate was neutral, and the obtained solid was dried in an oven at 80°C for 60 min to obtain Ce(SO 4 ) 2 Material.

[0058] The carbon-coated cerium phosphate composite materials provided in Examples 1-3 and the Ce(SO4) provided in Comparative Example 1 were tested as follows: 4 ) 2 Materials for effect verification:

[0059] 1. The carbon-coated cerium phosphate composite material provided in Example 1 was observed using a transmission electron microscope (Tecnai F20) to obtain the following microscopic morphology: Figure 1 .

[0060] Depend on Figure 1 It can be seen that in the carbon-coated cerium phosphate composite material provided in Example 1, the cerium phosphate nanoparticles are uniformly coated with carbon.

[0061] 2. The carbon-coated cerium phosphate composite material provided in Example 2 was subjected to crystal analysis using an X-ray diffractometer (SmartLab SE). The results are as follows: Figure 2 .

[0062] Depend on Figure 2 It can be seen that the composite material provided in Example 2 is carbon-coated cerium phosphate.

[0063] 3. Determination of the carbon-coated cerium phosphate composite materials provided in Examples 1-4 and the Ce(SO 4 ) 2 The degradation of methyl orange by the material under visible light. Figure 3 .

[0064] Depend on Figure 3It can be seen that the degradation rate of methyl orange of the carbon-coated cerium phosphate composite material provided in Example 1 after 45 minutes of visible light irradiation reaches 98.8%, the degradation rates of methyl orange of the carbon-coated cerium phosphate composite materials provided in Example 2, Example 3, and Example 4 after 45 minutes of visible light irradiation are 61.9%, 72.9%, and 30.9%, respectively, while the degradation rate of methyl orange of the cerium phosphate provided in Comparative Example 1 after 45 minutes of visible light irradiation is only 58.0%.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A carbon-coated cerium phosphate composite material, It is characterized in that The raw materials include the following parts by weight: 1-3 parts Ce(SO 4 ) 2 , 5-20 parts of pure water, 2-5 parts of 98% sulfuric acid, and 0.5-3 parts of 70% phytic acid solution.

2. A method for preparing the carbon-coated cerium phosphate composite material as claimed in claim 1, It is characterized in that The steps include: S1. Place Ce(SO 4 ) 2 Place in a beaker, add pure water and 98% sulfuric acid to dissolve, stir evenly to obtain a mixed solution A; S2, mixing 70% phytic acid solution with pure water to obtain a mixed solution B; S3, mixing solution A and solution B, stirring evenly, adjusting the pH value of the solution with a 20% by mass NaOH solution, and then transferring the mixed solution to a reactor for hydrothermal reaction; S4. Centrifuge or filter the mixture after the reaction, wash, dry and grind the obtained solid to obtain a composite material of carbon-coated cerium phosphate.

3. The preparation method according to claim 2, It is characterized in that In step S3, the pH value of the solution is adjusted to 2-11 using 20% ​​NaOH solution.

4. The preparation method according to claim 2, It is characterized in that In step S3, the mixed solution is transferred to a reaction kettle and subjected to a hydrothermal reaction at 70-180° C. for 6-12 hours.

5. The preparation method according to claim 2, It is characterized in that In step S4, the obtained solid is washed and then dried at 60-120° C. for 30-120 min.

6. Use of the carbon-coated cerium phosphate composite material according to claim 1 or the carbon-coated cerium phosphate composite material prepared by the preparation method according to any one of claims 2 to 5 as a photocatalytic material.