Composite photocatalyst with double heterojunctions as well as preparation method and application of composite photocatalyst
By constructing the NiCo-LDH@ZnCdS@Mo2C/rGO composite structure of type II heterojunction and Schottky junction in the photocatalyst, the problem of low photocatalyst efficiency is solved, and efficient photocatalytic water decomposition and hydrogen production is achieved. The rate is significantly improved and the stability of the catalyst is improved.
Patent Information
- Application Number
- CN202410971297.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing photocatalysts are inefficient in the process of photocatalyzed water hydrogen production, mainly due to the rapid recombination of photogenerated electrons and holes, narrow absorption range and product reverse reaction, resulting in low solar-hydrogen conversion efficiency and the scarcity of precious metal cocatalysts. and high costs limit its application.
NiCo-LDH@ZnCdS@Mo2C/rGO composite photocatalyst with Type II heterojunction and Schottky junction was prepared by metal ion etching method, and its energy band structure was regulated to accelerate electron transfer and separation, improve catalytic activity, and The coordinated action of the NiCo-LDH@ZnCdS heterojunction and the ZnCdS@Mo2C/rGO Schottky junction is formed to inhibit electron recombination.
The photocatalytic hydrogen production rate was significantly improved. The hydrogen production rate of NiCo-LDH@ZnCdS@Mo2C/rGO reached 90.1 mmol g–1 h–1, 2.5 times that of pure ZnCdS, enhancing the photostability and reusability of the catalyst. .
Smart Images

Figure CN118904374A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite photocatalyst with a double heterojunction and a preparation method and application thereof, belonging to the technical field of photocatalytic decomposition of water to produce hydrogen. Background Art
[0002] With the depletion of fossil energy and the continuous growth of global energy demand, the development of renewable energy has become a top priority. Hydrogen energy, as a clean and efficient energy with abundant reserves, safety, no pollution, and high energy density, has become an ideal substitute for fossil energy. Among the existing hydrogen production technologies, solar energy, as a continuous, safe, harmless energy with huge reserves, makes photocatalytic water hydrogen production technology have a natural advantage. However, due to the rapid recombination of photogenerated electrons and holes, the narrow absorption range of photocatalysts for sunlight and insufficient utilization, and the rapid reverse reaction of the products H2 and O2 on the catalyst surface, the solar energy-hydrogen energy conversion efficiency of pure semiconductor photocatalysts is too low and does not have a competitive advantage. Therefore, the development of photocatalyst materials with excellent performance is the biggest challenge for photocatalytic hydrogen production at present.
[0003] The performance of photocatalysts can be improved through strategies such as morphology regulation, heterostructure construction, element doping, and co-catalyst modification. Among them, co-catalyst modification has been widely studied because it helps to reduce the recombination of photogenerated carriers, provide reaction sites, and reduce the activation energy of the reaction. Precious metals are currently the most efficient and stable co-catalysts, such as Pt, Pd, Au, etc., but their scarcity and high cost limit their large-scale application. The development of inexpensive and readily available non-precious metal co-catalysts has become a current research hotspot. Transition metal carbides have advantages such as electronic structure similar to Pt, high conductivity, wide pH range and good stability. They show excellent co-catalytic hydrogen evolution activity and are ideal substitutes for Pt-based precious metal co-catalysts. At the same time, the two semiconductors with staggered band structures are closely contacted to construct a heterojunction. Due to the different energy levels of the semiconductors on both sides of the interface, a potential difference is generated, inducing the formation of a built-in electric field, thereby accelerating the separation of photogenerated carriers in the space charge region and enhancing the activity of the photocatalytic reaction. By constructing a heterojunction and modifying the co-catalyst at the same time to build a double heterostructure, the photocatalytic hydrogen production activity can be further improved through the synergistic effect of the heterojunction and the co-catalyst. Especially for the composite of LDH nanosheets, CdS and co-catalysts, the traditional hydrothermal method is often used to prepare LDH nanosheets, whose band structure satisfies the transfer of photogenerated electrons from CdS to LDH nanosheets and then to the co-catalyst. Not only is the driving force for the transfer of photogenerated electrons limited, but CdS is still in the outermost layer and is still severely corroded by light. Summary of the invention
[0004] In view of the problem that the current transition metal carbide co-catalyst has limited ability to enhance the semiconductor photocatalytic hydrogen production performance, the present invention provides a double heterojunction composite photocatalyst having both a type II heterojunction and a Schottky junction, and the present invention also provides a preparation method and application of the catalyst.
[0005] The present invention provides a double heterojunction composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO having both type II heterojunction NiCo-LDH@ZnCdS and Schottky junction ZnCdS@Mo2C / rGO. Different from the traditional hydrothermal method for preparing LDH nanosheets, the present invention prepares NiCo-LDH nanocages by metal ion etching, regulates its band structure, and reduces the Fermi levels of NiCo-LDH, ZnCdS, and Mo2C in sequence. In the composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO, the built-in electric field at the type II heterojunction NiCo-LDH@ZnCdS interface and the built-in electric field at the Schottky junction ZnCdS@Mo2C / rGO interface are in the same direction, so that NiCo-LDH acts as a propeller to drive more electrons to transfer to Mo2C along the cascade electron transfer channel, thereby accelerating electron transfer and improving the utilization rate of photogenerated electrons. At the same time, a high Schottky barrier is retained to effectively inhibit electron backflow and improve the separation efficiency of photogenerated carriers, thereby enhancing the photocatalytic reaction activity; and the good photocorrosion resistance of the LDH nanocage protects ZnCdS, improves its photostability, and thus improves the reusability of the composite catalyst.
[0006] The present invention provides a composite photocatalyst with a double heterojunction, using reduced graphene oxide with uniformly dispersed ultrafine Mo2C nanoparticles as a substrate, in-situ loading ZnCdS by a hydrothermal method to obtain ZnCdS@Mo2C / rGO, further growing ZIF-67 on the surface of ZnCdS@Mo2C / rGO, and 2+ Hollow nanocage-like NiCo-LDH was obtained by etching, thus constructing a NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst. Through the synergistic effect of NiCo-LDH@ZnCdS heterojunction and ZnCdS@Mo2C / rGO Schottky junction, a cascade electron transfer channel was formed, which accelerated the transfer of photogenerated electrons to Mo2C and inhibited the recombination of photogenerated carriers, thereby improving the photocatalytic hydrogen production performance.
[0007] The present invention provides a method for preparing the composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO having a double heterojunction, comprising the following steps: In the first step, Mo2C / rGO was used as a carrier, and zinc source, cadmium source and sulfur source were added to hydrothermally load ZnCdS in situ to obtain ZnCdS@Mo2C / rGO photocatalyst with Schottky junction. In the second step, cobalt nitrate and 2-methylimidazole were added to grow rhombic dodecahedron Co-ZIF on the surface of ZnCdS@Mo2C / rGO; In the third step, nickel nitrate was added and Co-ZIF was hydrothermally etched to obtain hollow nanocage-shaped NiCo-ZIF in situ, and a heterojunction was constructed with ZnCdS to obtain a NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst with a double heterojunction.
[0008] In the above preparation method, the cadmium source is any one of cadmium chloride, cadmium nitrate and cadmium acetate; the zinc source is any one of zinc chloride, zinc nitrate and zinc acetate; and the sulfur source is any one of thiourea, sodium sulfide and thioacetamide.
[0009] The preparation method of the composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO with double heterojunction is as follows: (1) 0.01-0.05 g of Mo2C / rGO was ultrasonically dispersed in 30-35 mL of deionized water, and 0.5-3.0 g of cadmium source, 0.5-3.0 g of zinc source, 0.2-3.0 g of sulfur source and 1-10 mL of NaOH solution (4 M) were added. After stirring for 1 h to fully dissolve the cadmium source, the cadmium source was hydrothermally heated at 120-200 °C for 6-24 h to obtain a ZnCdS@Mo2C / rGO composite photocatalyst with a Schottky junction. (2) 0.01-0.3 g of ZnCdS@Mo2C / rGO and 0.01-0.15 g of cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL of anhydrous methanol, marked as solution A. (3) Dissolve 0.01-0.15 g of 2-methylimidazole in another 20 mL of anhydrous methanol and label it as solution B. (4) mixing solution A of step (2) and solution B of step (3), stirring at room temperature for 2-24 h, washing with alcohol, and drying to obtain Co-ZIF@ZnCdS@Mo2C / rGO; (5) The Co-ZIF@ZnCdS@Mo2C / rGO obtained in step (4) was ultrasonically dispersed in 30 mL of anhydrous ethanol and marked as solution C; (6) Dissolve 0.003-0.05 g of nickel nitrate hexahydrate in another 10 mL of anhydrous ethanol and label it as solution D. (7) The solution C of step (5) and the solution D of step (6) are mixed and hydrothermally treated at 80-160° C. for 0.5-12 h to obtain a NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst having a double heterostructure.
[0010] The present invention provides a double heterojunction composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO having both type II heterojunction NiCo-LDH@ZnCdS and Schottky junction ZnCdS@Mo2C / rGO. Firstly, ZnCdS is hydrothermally loaded on the Mo2C / rGO co-catalyst to construct the ZnCdS@Mo2C / rGO Schottky junction. Then, a rhombic dodecahedron Co-ZIF is grown on the surface of ZnCdS@Mo2C / rGO, and Ni is introduced. 2+ Hollow nanocage NiCo-LDH was obtained by hydrothermal etching, and type II heterojunction NiCo-LDH@ZnCdS was constructed with ZnCdS. Through the rational design of the catalyst structure, the directions of the built-in electric fields at the interface of heterojunction NiCo-LDH@ZnCdS and Schottky junction ZnCdS@Mo2C / rGO are consistent. Under the synergistic effect of NiCo-LDH@ZnCdS heterojunction and ZnCdS@Mo2C / rGO Schottky junction, NiCo-LDH acts as a propeller to push more photogenerated electrons on ZnCdS to transfer to Mo2C / rGO. At the same time, the higher Schottky barrier of ZnCdS@Mo2C / rGO prevents electron backflow, forming a cascade electron transfer channel, inhibiting the recombination of photogenerated carriers, and improving the separation efficiency and effective utilization of photogenerated electrons, thereby improving the photocatalytic water decomposition and hydrogen production performance of ZnCdS. Moreover, the hollow nanocage-like structure of NiCo-LDH can prevent the agglomeration of layered double hydroxides and fully expose more active sites, which is beneficial to electron transfer.
[0011] The present invention provides the application of the composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO with double heterojunction in photocatalytic water decomposition and hydrogen production. A 300 W xenon lamp (with a 400 nm filter) is used as the light source, and the reaction is carried out in a sacrificial system of 0.35 M Na2S / 0.25 M Na2SO3 with 100 mL added. The hydrogen production rate of pure ZnCdS is 36.1 mmol g –1 h –1 The hydrogen production rate of ZnCdS@Mo2C / rGO Schottky junction is 52.8 mmol g –1 h –1 The hydrogen production rate of NiCo-LDH@ZnCdS type II heterojunction is 51.7 mmol g –1 h –1 The hydrogen production rate of NiCo-LDH@ZnCdS@Mo2C / rGO with both type II heterojunction and Schottky junction is 90.1 mmol g –1 h –1, which is 1.7 times that of the ZnCdS@Mo2C / rGO Schottky junction and 2.5 times that of pure ZnCdS, fully demonstrating the superiority of the catalyst of the present invention.
[0012] Beneficial effects of the present invention: (1) The establishment of the double heterojunction in NiCo-LDH@ZnCdS@Mo2C / rGO not only improves the transfer of electrons at the interface of NiCo-LDH@ZnCdS and ZnCdS@Mo2C / rGO through the action of the built-in electric field at the interface, but also because the electric field directions of the two built-in electric fields are consistent, they can work synergistically, allowing NiCo-LDH to act as a propeller to push more disordered electrons in ZnCdS to be transferred in an orderly manner to the interface of ZnCdS@Mo2C / rGO, and then transferred to Mo2C / rGO for reduction and hydrogen production. At the same time, the rectifying effect of the ZnCdS@Mo2C / rGO Schottky heterojunction can prevent the electrons transferred to Mo2C / rGO from flowing back to ZnCdS, promoting the cascade transfer of electrons along the NiCo-LDH→ZnCdS→Mo2C path, optimizing the utilization rate of photogenerated carriers, and thus improving the reaction activity; (2) The hollow nanocage-structured NiCo-LDH was prepared by etching ZIF with metal salts. In terms of morphology, it can effectively avoid the disadvantage of layered double hydroxides being easily agglomerated and stacked, and has a large specific surface area, fully exposing more active sites, which is conducive to electron transfer; in terms of energy band structure, it can regulate its energy band structure, making its Fermi level significantly higher than that of ZnCdS, constructing a type II heterojunction, and promoting electron transfer. Ultimately, the hydrogen production rate of the composite photocatalyst reached 90.1 mmolg –1 h –1 , which is 2.5 times the hydrogen production performance of pure ZnCdS.
[0013] In order to illustrate the structure of the composite photocatalyst with double heterojunction prepared by the present invention and the photocatalytic water decomposition and hydrogen evolution performance, further description is given in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 XRD and FT-IR spectra of Mo2C / rGO, ZnCdS@Mo2C / rGO, Co-ZIF@ZnCdS@Mo2C / rGO and NiCo-LDH@ZnCdS@Mo2C / rGO samples prepared in Example 1.
[0015] Figure 2 SEM images of Mo2C / rGO, ZnCdS@Mo2C / rGO, Co-ZIF@ZnCdS@Mo2C / rGO and NiCo-LDH@ZnCdS@Mo2C / rGO samples prepared in Example 1.
[0016] Figure 3 This is the HR-TEM spectrum of the NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst prepared in Example 1.
[0017] Figure 4 It is a comparison chart of the photocatalytic hydrogen production performance of Examples 1-5.
[0018] Figure 5 It is a comparison chart of the photocatalytic hydrogen production performance of Example 1 and Comparative Examples 1-4.
[0019] Figure 6 This is a comparison chart of the photocatalytic hydrogen production performance of Example 1 and Comparative Example 5. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and the disclosure and materials cited therein are hereby incorporated by reference.
[0022] Technical equivalents to the specific embodiments described that are apparent to those skilled in the art using no more than routine experimentation are intended to be encompassed by this application.
[0023] The experimental methods in the following examples are all conventional methods unless otherwise specified. The instruments and equipment used in the following examples are all conventional laboratory instruments and equipment unless otherwise specified; the experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.
[0024] (i) The following example illustrates the preparation of a composite photocatalyst loaded with a double transition metal carbide co-catalyst. Example 1
[0025] 0.015 g Mo2C / rGO was ultrasonically dispersed in 30 mL deionized water, 1.32 g zinc acetate dihydrate and 1.60 g cadmium acetate dihydrate were added, and stirred for 10 min to fully dissolve in the Mo2C / rGO solution, followed by 1.1 g thioacetamide and 6 mL of 4 M NaOH solution, and stirred for 1 h. Then, the mixed solution was transferred to a high-pressure reactor and hydrothermal at 180 °C for 12 h to obtain ZnCdS@Mo2C / rGO.
[0026] 0.1 g ZnCdS@Mo2C / rGO and 0.044 g cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL anhydrous methanol, marked as solution A. At the same time, 0.05 g 2-methylimidazole was dissolved in another 20 mL anhydrous methanol, marked as solution B. Solutions A and B were quickly mixed, stirred at room temperature for 2 h, centrifuged, washed with alcohol, and dried to obtain Co-ZIF@ZnCdS@Mo2C / rGO composite.
[0027] The Co-ZIF@ZnCdS@Mo2C / rGO obtained above was ultrasonically dispersed in 30 mL of anhydrous ethanol again, marked as solution C. At the same time, 0.005 g of nickel nitrate hexahydrate was ultrasonically dissolved in 10 mL of anhydrous ethanol, marked as solution D. Solutions C and D were mixed and stirred evenly. Then, it was transferred to a high-pressure reactor and hydrothermal at 90 °C for 1 h to obtain a hollow nanocage-shaped NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst.
[0028] Figure 1 XRD (a) and FT-IR (b) spectra of Mo2C / rGO, ZnCdS@Mo2C / rGO, Co-ZIF@ZnCdS@Mo2C / rGO and NiCo-LDH@ZnCdS@Mo2C / rGO samples prepared in Example 1. The spectra show that the hydrothermally prepared ZnCdS is a ZnCdS solid solution, not a physical mixture of ZnS and CdS. After the growth of Co-ZIF on the surface of ZnCdS@Mo2C / rGO, an obvious Co-ZIF peak appears, while on the surface of Ni 2+ After etching, the ZIF peak disappeared, proving that the ZIF structure was destroyed to form NiCo-LDH, indicating the successful preparation of NiCo-LDH@ZnCdS@Mo2C / rGO.
[0029] Figure 2SEM images of Mo2C / rGO (a), ZnCdS@Mo2C / rGO (b), Co-ZIF@ZnCdS@Mo2C / rGO (c), and NiCo-LDH@ZnCdS@Mo2C / rGO (d) samples prepared in Example 1. It can be clearly seen from the figure that the surface of Mo2C / rGO is smooth and the lateral size is wide; after loading ZnCdS, a layer of nanoparticles is coated on the surface; after further growth of Co-ZIF on the surface of ZnCdS@Mo2C / rGO, an obvious rhombic dodecahedron structure appears, and the surface is smooth; through Ni 2+ After etching, it turned into hexagons with rough surfaces, proving the destruction of ZIF.
[0030] Figure 3 This is the HR-TEM spectrum of the NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst prepared in Example 1. The crystal planes with lattice spacings of 0.32 nm, 0.22 nm, and 0.28 nm correspond to the ZnCdS (111) crystal plane, Mo2C (101) crystal plane, and NiCo-LDH (100) crystal plane, respectively, which once again confirms the successful preparation of NiCo-LDH@ZnCdS@Mo2C / rGO. Example 2
[0031] 0.01 g Mo2C / rGO was ultrasonically dispersed in 30 mL deionized water, 1.0 g zinc nitrate hexahydrate and 1.0 g cadmium nitrate tetrahydrate were added, and stirred for 10 min to fully dissolve in the Mo2C / rGO solution, followed by 0.5 g thiourea and 4 mL of 4M NaOH solution, and stirred for 1 h. Then, the mixed solution was transferred to a high-pressure reactor and hydrothermally heated at 120 °C for 6 h to obtain ZnCdS@Mo2C / rGO.
[0032] 0.05 g ZnCdS@Mo2C / rGO and 0.01 g cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL anhydrous methanol, marked as solution A. At the same time, 0.01 g 2-methylimidazole was dissolved in another 20 mL anhydrous methanol, marked as solution B. Solutions A and B were quickly mixed, stirred at room temperature for 12 h, centrifuged, washed with alcohol, and dried to obtain Co-ZIF@ZnCdS@Mo2C / rGO composite.
[0033] The Co-ZIF@ZnCdS@Mo2C / rGO obtained above was ultrasonically dispersed in 30 mL of anhydrous ethanol again, marked as solution C. At the same time, 0.003 g of nickel nitrate hexahydrate was ultrasonically dissolved in 10 mL of anhydrous ethanol, marked as solution D. Solutions C and D were mixed and stirred evenly. Then, it was transferred to a high-pressure reactor and hydrothermal at 80 °C for 0.5 h to obtain a hollow nanocage-shaped NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst. Example 3
[0034] Weigh 0.03 g Mo2C / rGO and ultrasonically disperse it in 30 mL deionized water, add 2.0 g zinc chloride and 2.0 g cadmium chloride, stir for 10 min to fully dissolve them in the Mo2C / rGO solution, then add 1.5 g sodium sulfide and 8 mL of 4 MNaOH solution and stir for 1 h. Then, transfer the mixed solution to a high-pressure reactor and hydrothermally heat it at 200 °C for 24 h to obtain ZnCdS@Mo2C / rGO.
[0035] 0.15 g ZnCdS@Mo2C / rGO and 0.07 g cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL anhydrous methanol, marked as solution A. At the same time, 0.08 g 2-methylimidazole was dissolved in another 20 mL anhydrous methanol, marked as solution B. Solutions A and B were quickly mixed, stirred at room temperature for 24 h, centrifuged, washed with alcohol, and dried to obtain Co-ZIF@ZnCdS@Mo2C / rGO composite.
[0036] The Co-ZIF@ZnCdS@Mo2C / rGO obtained above was ultrasonically dispersed in 30 mL of anhydrous ethanol again, marked as solution C. At the same time, 0.01 g of nickel nitrate hexahydrate was ultrasonically dissolved in 10 mL of anhydrous ethanol, marked as solution D. Solutions C and D were mixed and stirred evenly. Then, it was transferred to a high-pressure reactor and hydrothermal at 160 °C for 12 h to obtain a hollow nanocage-shaped NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst. Example 4
[0037] 0.02 g Mo2C / rGO was ultrasonically dispersed in 30 mL deionized water, 1.50 g zinc acetate dihydrate and 1.50 g cadmium acetate dihydrate were added, and stirred for 10 min to fully dissolve in the Mo2C / rGO solution, followed by 1.1 g thiourea and 5 mL of 4 M NaOH solution, and stirred for 1 h. Then, the mixed solution was transferred to a high-pressure reactor and hydrothermal at 160 °C for 16 h to obtain ZnCdS@Mo2C / rGO.
[0038] 0.12 g ZnCdS@Mo2C / rGO and 0.06 g cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL anhydrous methanol, marked as solution A. At the same time, 0.06 g 2-methylimidazole was dissolved in another 20 mL anhydrous methanol, marked as solution B. Solutions A and B were quickly mixed, stirred at room temperature for 2 h, centrifuged, washed with alcohol, and dried to obtain Co-ZIF@ZnCdS@Mo2C / rGO composite.
[0039] The Co-ZIF@ZnCdS@Mo2C / rGO obtained above was ultrasonically dispersed in 30 mL of anhydrous ethanol again, marked as solution C. At the same time, 0.007 g of nickel nitrate hexahydrate was ultrasonically dissolved in 10 mL of anhydrous ethanol, marked as solution D. Solutions C and D were mixed and stirred evenly. Then, it was transferred to a high-pressure reactor and hydrothermal at 120 °C for 2 h to obtain a hollow nanocage-shaped NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst. Example 5
[0040] Weigh 0.015 g Mo2C / rGO and ultrasonically disperse it in 30 mL deionized water, add 2.0 g zinc acetate dihydrate and 2.0 g cadmium acetate dihydrate, stir for 10 min to fully dissolve them in the Mo2C / rGO solution, then add 1.5 g sodium sulfide and 4 mL of 4 M NaOH solution and stir for 1 h. Then, transfer the mixed solution to a high-pressure reactor and hydroheat it at 140 °C for 24 h to obtain ZnCdS@Mo2C / rGO.
[0041] 0.1 g ZnCdS@Mo2C / rGO and 0.07 g cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL anhydrous methanol, marked as solution A. At the same time, 0.08 g 2-methylimidazole was dissolved in another 20 mL anhydrous methanol, marked as solution B. Solutions A and B were quickly mixed, stirred at room temperature for 6 h, centrifuged, washed with alcohol, and dried to obtain Co-ZIF@ZnCdS@Mo2C / rGO composite.
[0042] The Co-ZIF@ZnCdS@Mo2C / rGO obtained above was ultrasonically dispersed in 30 mL of anhydrous ethanol again, marked as solution C. At the same time, 0.01 g of nickel nitrate hexahydrate was ultrasonically dissolved in 10 mL of anhydrous ethanol, marked as solution D. Solutions C and D were mixed and stirred evenly. Then, it was transferred to a high-pressure reactor and hydrothermal at 140 °C for 6 h to obtain a hollow nanocage-shaped NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst.
[0043] Comparative Example 1: 0.015 g Mo2C / rGO was ultrasonically dispersed in 30 mL deionized water, 1.32 g zinc acetate dihydrate and 1.60 g cadmium acetate dihydrate were added, and stirred for 10 min to fully dissolve in the Mo2C / rGO solution, followed by 1.1 g thioacetamide and 6 mL of 4 M NaOH solution, and stirred for 1 h. Then, the mixed solution was transferred to a high-pressure reactor and hydrothermal at 180 °C for 12 h to obtain ZnCdS@Mo2C / rGO.
[0044] Comparative Example 2: 1.32 g zinc acetate dihydrate and 1.60 g cadmium acetate dihydrate were weighed and dissolved in 30 mL deionized water, stirred for 10 min to fully dissolve, and then 1.1 g thioacetamide and 6 mL 4 M NaOH solution were added and stirred for 1 h. Then, the mixed solution was transferred to a high-pressure reactor and hydrothermal at 180 °C for 12 h to obtain ZnCdS.
[0045] Comparative Example 3: 1.32 g zinc acetate dihydrate and 1.60 g cadmium acetate dihydrate were weighed and dissolved in 30 mL deionized water, stirred for 10 min to fully dissolve, and then 1.1 g thioacetamide and 6 mL 4 M NaOH solution were added and stirred for 1 h. Then, the mixed solution was transferred to a high-pressure reactor and hydrothermal at 180 °C for 12 h to obtain ZnCdS.
[0046] 0.1 g ZnCdS and 0.044 g cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL anhydrous methanol, marked as solution A. At the same time, 0.05 g 2-methylimidazole was dissolved in another 20 mL anhydrous methanol, marked as solution B. Solutions A and B were quickly mixed, stirred at room temperature for 2 h, centrifuged, washed with alcohol, and dried to obtain the Co-ZIF@ZnCdS composite.
[0047] The Co-ZIF@ZnCdS obtained above was ultrasonically dispersed in 30 mL of anhydrous ethanol again, marked as solution C. At the same time, 0.005 g of nickel nitrate hexahydrate was ultrasonically dissolved in 10 mL of anhydrous ethanol, marked as solution D. Solutions C and D were mixed and stirred evenly. Then, they were transferred to a high-pressure reactor and hydrothermal at 90 °C for 1 h to obtain a hollow nanocage-shaped NiCo-LDH@ZnCdS composite photocatalyst.
[0048] Comparative Example 4: 0.044 g of cobalt nitrate hexahydrate was ultrasonically dispersed in 20 mL of anhydrous methanol, marked as solution A. At the same time, 0.05 g of 2-methylimidazole was dissolved in another 20 mL of anhydrous methanol, marked as solution B. Solutions A and B were quickly mixed, stirred at room temperature for 2 h, centrifuged, washed with alcohol, and dried to obtain Co-ZIF.
[0049] The Co-ZIF obtained above was ultrasonically dispersed in 30 mL of anhydrous ethanol again, marked as solution C. At the same time, 0.005 g of nickel nitrate hexahydrate was ultrasonically dissolved in 10 mL of anhydrous ethanol, marked as solution D. Solutions C and D were mixed and stirred evenly. Then, it was transferred to a high-pressure reactor and hydrothermal at 90 °C for 1 h to obtain hollow nanocage-shaped NiCo-LDH.
[0050] Comparative Example 5: 0.015 g Mo2C / rGO was ultrasonically dispersed in 30 mL deionized water, 1.32 g zinc acetate dihydrate and 1.60 g cadmium acetate dihydrate were added, and stirred for 10 min to fully dissolve in the Mo2C / rGO solution, followed by 1.1 g thioacetamide and 6 mL of 4 M NaOH solution, and stirred for 1 h. Then, the mixed solution was transferred to a high-pressure reactor and hydrothermal at 180 °C for 12 h to obtain ZnCdS@Mo2C / rGO.
[0051] The above 0.1 g ZnCdS@Mo2C / rGO, 0.044 g cobalt nitrate hexahydrate and 0.031 g nickel nitrate hexahydrate were ultrasonically dispersed in 40 mL deionized water and stirred at room temperature for 30 min. Then 0.010 g ammonium fluoride and 0.038 g urea were added and stirred for 30 min. Then, the mixture was transferred to a polytetrafluoroethylene liner and hydroheated at 120 °C for 12 h to obtain NiCo-LDH nanosheets@ZnCdS@Mo2C / rGO.
[0052] (II) Photocatalytic hydrogen production performance of the composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO in the present invention The evaluation was conducted using a top-illuminated Pyrex glass reactor. Weigh 0.035 g of the photocatalyst of Example 1, disperse it in 100 mL of a 0.35 M Na2S / 0.25 M Na2SO3 mixed solution, place it in a reactor, connect the reaction device, keep the temperature of the reaction system at 6°C, and use a 300 W xenon lamp (with a 400 nm filter) as the light source under magnetic stirring to evaluate the performance of photocatalytic decomposition of water to produce hydrogen. Before starting the reaction, evacuate the reaction system for 30 minutes to completely remove the air in the system. The amount of hydrogen produced by the reaction was quantitatively analyzed using a gas chromatograph equipped with a thermal conductivity detector.
[0053] The same method as above was used to test the catalytic hydrogen production performance of the hollow nanocage structure NiCo-LDH@ZnCdS@Mo2C / rGO photocatalyst obtained in Examples 2-5. Figure 4 As shown in Figure 1, the hydrogen production performance of NiCo-LDH@ZnCdS@Mo2C / rGO in Example 1 is as high as 90.1 mmol g –1 h –1 The hydrogen production performances of Examples 2-5 are 60.7, 73.5, 65.3, and 70.6 mmol g, respectively. –1 h –1 , which are lower than those in Example 1, but still significantly higher than those in Comparative Examples 1-4.
[0054] The same method as above was used to test the catalytic hydrogen production performance of the photocatalysts ZnCdS@Mo2C / rGO, ZnCdS, NiCo-LDH@ZnCdS, NiCo-LDH and NiCo-LDH nanosheets@ZnCdS@Mo2C / rGO obtained in Comparative Examples 1-5.
[0055] like Figure 5 As shown in Figure 1, the hydrogen production performance of NiCo-LDH nanocage @ZnCdS@Mo2C / rGO in Example 1 is as high as 90.1 mmolg –1 h –1 , which are 2.5 and 1.7 times the hydrogen production performance of pure ZnCdS and ZnCdS@Mo2C / rGO, respectively, indicating that the composite photocatalyst NiCo-LDH nanocage@ZnCdS@Mo2C / rGO prepared by the present invention has excellent photocatalytic water decomposition and hydrogen production performance. Obviously, the hydrogen production performance of NiCo-LDH nanocage@ZnCdS@Mo2C / rGO is better than that of NiCo-LDH nanosheet@ZnCdS@Mo2C / rGO (Comparative Example 5, 60.3 mmol g –1 h –1 )、NiCo-LDH nanocage@ZnCdS (Comparative Example 3, 51.7 mmol g –1 h –1 )、ZnCdS@Mo2C / rGO(Comparative Example 1, 52.8 mmol g –1 h –1 )、ZnCdS(Comparative Example 2,36.1 mmol g –1 h –1), while the hydrogen production of NiCo-LDH (Comparative Example 4) is almost zero, indicating that the synergistic effect of the NiCo-LDH@ZnCdS heterojunction and the ZnCdS@Mo2C / rGO Schottky junction in NiCo-LDH@ZnCdS@Mo2C / rGO can promote the effective separation of photogenerated electrons and greatly enhance the photocatalytic hydrogen production performance of ZnCdS.
[0056] In addition, if Figure 6 As shown in the figure, the hydrogen production performance of NiCo-LDH nanocage @ ZnCdS @ Mo2C / rGO is better than that of NiCo-LDH nanosheet @ ZnCdS @ Mo2C / rGO (Comparative Example 5), which proves the superiority of the NiCo-LDH nanocage @ ZnCdS @ Mo2C / rGO structure. In NiCo-LDH nanocage @ ZnCdS @ Mo2C / rGO, since the directions of the built-in electric fields at the interface of the NiCo-LDH nanocage @ ZnCdS heterojunction and the ZnCdS @ Mo2C / rGO Schottky junction are consistent, the NiCo-LDH nanocage acts as a propeller to push more photogenerated electrons in ZnCdS to transfer to Mo2C / rGO, which not only improves the separation efficiency of photogenerated carriers, but also greatly promotes the effective utilization of photogenerated electrons, thereby improving the photocatalytic hydrogen production activity. However, the band structure of NiCo-LDH nanosheets cannot make the direction of the built-in electric field at the interface of NiCo-LDH nanosheets@ZnCdS heterojunction and ZnCdS@Mo2C / rGO Schottky junction consistent. Therefore, it cannot promote the transfer of more photogenerated electrons, and the hydrogen production performance is weaker than that of NiCo-LDH nanocages@ZnCdS@Mo2C / rGO.
[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite photocatalyst with a double heterojunction, characterized in that: Using reduced graphene oxide with uniformly dispersed ultrafine Mo2C nanoparticles as the substrate, ZnCdS was in situ loaded by a hydrothermal method to obtain ZnCdS@Mo2C / rGO. Then, rhombic dodecahedral Co-ZIF was grown on the surface of ZnCdS@Mo2C / rGO. 2+ NiCo-LDH with a hollow nanocage structure was obtained by etching, and a NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst was constructed; through the synergistic effect of the NiCo-LDH@ZnCdS heterojunction and the ZnCdS@Mo2C / rGO Schottky junction, a cascade electron transfer channel was formed, which accelerated the transfer of photogenerated electrons to Mo2C, inhibited the recombination of photogenerated carriers, and improved the photocatalytic hydrogen production performance.
2. A method for preparing a composite photocatalyst having a double heterojunction according to claim 1, characterized in that The following steps are involved: In the first step, Mo2C / rGO was used as a carrier, and zinc source, cadmium source and sulfur source were added to hydrothermally load ZnCdS in situ to obtain ZnCdS@Mo2C / rGO photocatalyst with Schottky junction. In the second step, cobalt nitrate and 2-methylimidazole were added to grow rhombic dodecahedron Co-ZIF on the surface of ZnCdS@Mo2C / rGO; In the third step, nickel nitrate was added and Co-ZIF was hydrothermally etched to obtain hollow nanocage-shaped NiCo-ZIF in situ, and a heterojunction was constructed with ZnCdS to obtain a NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst with a double heterojunction.
3. The method for preparing a composite photocatalyst having a double heterojunction according to claim 2, characterized in that: The cadmium source is any one of cadmium chloride, cadmium nitrate and cadmium acetate; the zinc source is any one of zinc chloride, zinc nitrate and zinc acetate; the sulfur source is any one of thiourea, sodium sulfide and thioacetamide.
4. The method for preparing a composite photocatalyst having a double heterojunction according to claim 2, characterized in that: The specific steps are as follows: (1) 0.01-0.05 g of Mo2C / rGO was ultrasonically dispersed in 30-35 mL of deionized water, and 0.5-3.0 g of cadmium source, 0.5-3.0 g of zinc source, 0.2-3.0 g of sulfur source and 1-10 mL of NaOH solution were added. After stirring for 1 h to fully dissolve the cadmium source, the cadmium source was hydrothermally heated at 120-200 °C for 6-24 h to obtain a ZnCdS@Mo2C / rGO composite photocatalyst with a Schottky junction. (2) 0.01-0.3 g of ZnCdS@Mo2C / rGO and 0.01-0.15 g of cobalt nitrate hexahydrate were ultrasonically dispersed in 20 mL of anhydrous methanol, marked as solution A. (3) Dissolve 0.01-0.15 g of 2-methylimidazole in another 20 mL of anhydrous methanol and label it as solution B. (4) mixing solution A of step (2) and solution B of step (3), stirring at room temperature for 2-24 h, washing with alcohol, and drying to obtain Co-ZIF@ZnCdS@Mo2C / rGO; (5) The Co-ZIF@ZnCdS@Mo2C / rGO obtained in step (4) was ultrasonically dispersed in 30 mL of anhydrous ethanol and marked as solution C; (6) Dissolve 0.003-0.05 g of nickel nitrate hexahydrate in another 10 mL of anhydrous ethanol and label it as solution D. (7) The solution C of step (5) and the solution D of step (6) are mixed and hydrothermally treated at 80-160° C. for 0.5-12 h to obtain a NiCo-LDH@ZnCdS@Mo2C / rGO composite photocatalyst having a double heterostructure.
5. The method for preparing a composite photocatalyst having a double heterojunction according to claim 4, characterized in that: In step (1), the concentration of the NaOH solution is 4 M.
6. Use of the composite photocatalyst with double heterojunction as claimed in claim 1 in photocatalytic decomposition of water to produce hydrogen.
7. The use according to claim 6, characterized in that: A 300 W xenon lamp was used as the light source, and the reaction was carried out in a sacrificial system containing 100 mL of 0.35 M Na2S / 0.25 M Na2SO3.
8. The use according to claim 6, characterized in that: The composite photocatalyst NiCo-LDH@ZnCdS@Mo2C / rGO with double heterojunction can produce hydrogen at a rate of 90.1 mmol g –1 h –1 .
Citation Information
Patent Citations
Mo2C / CdS composite photocatalyst, and preparation and applications thereof
CN104959158A
Nickel-cobalt double metal oxide@nitrogen-oxygen co-doped carbon material / CdS photocatalytic material, preparation method and application thereof
CN110327962A
ZnCdS and MoS2 composite photocatalyst as well as preparation method and application thereof
CN116870934A
Layered double-metal hydroxide hollow nanocage catalyst as well as preparation method and application thereof
CN118147696A
RGO-Mo2C / MoC-rGO sodium ion battery composite negative electrode material and preparation method thereof
CN118281206A