Post-curing method for 3D thin-wall shell-shaped product

By using a combination of plasma air flow and ultraviolet light on 3D printed thin-walled shell products, the temperature during the post-curing process is controlled, and the problem of heat generated by photoinitiator reaction is solved, achieving uniform curing and improving the accuracy of the product.

CN118906460AActive Publication Date: 2024-11-08SHANGHAI COHERZ TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411178479.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-08
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

During 3D printing, especially when digital light processing technology is used, the heat generated by the photoinitiator reaction during the post-curing process is difficult to effectively dissipate, resulting in uneven expansion or shrinkage of the material, affecting product accuracy and transparency.

Method used

The surface of the thin-walled shell-like product completed by 3D printing is continuously sprayed with plasma air flow of 8℃ to 12℃. Combined with the light-initiation method of ultraviolet light, the reaction temperature of the post-curing process is controlled within the interval of 0℃ to 20℃, and plasma is used. The airflow takes away heat and avoids the generation of temperature gradients.

Benefits of technology

It effectively avoids uneven expansion or shrinkage of the material, ensures the accuracy and transparency of the product, reduces deformation and whitening color, and improves the quality of the final product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906460A_ABST
    Figure CN118906460A_ABST
Patent Text Reader

Abstract

The invention provides a post-curing method for a 3D thin-wall shell-shaped product, and belongs to the field of 3D printing, and the post-curing method specifically comprises the steps that plasma airflow at the temperature of 8-12 DEG C is used for conducting continuous spraying on the surface of the 3D-printed thin-wall shell-shaped product in a post-curing box for preset time, and the proportion of nitrogen in the plasma airflow is not smaller than 95%; the thin-wall shell-shaped product is subjected to post-curing in a photo-initiation mode through ultraviolet light, the reaction temperature of the whole post-curing process ranges from 0 DEG C to 20 DEG C, and plasma airflow is kept at the preset speed in the post-curing process; and after post-curing is completed, turning off the ultraviolet lamp, then turning off the plasma equipment, and taking out the thin-wall shell-shaped product. By means of the treatment scheme, the reaction temperature of the product in the whole post-curing process can be controlled within the preset interval, heat generated by violent reaction can be rapidly taken away, and therefore deformation is reduced as much as possible while the physical performance of the product is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of 3D printing, and in particular to a post-curing method for a 3D thin-wall shell-shaped product. Background Art

[0002] In 3D printing, especially when using digital light processing (DLP) technology, post-curing is a common key step in the industry. Through light initiation or thermal initiation, the unreacted resin is further polymerized to improve the reaction integrity of the matrix material and enhance the physical and chemical properties of the printed part. The common post-curing method is to use light of a certain wavelength (such as 205-460nm) and certain lighting parameters to trigger the photoinitiator in the residual resin after 3D printing to react.

[0003] However, to obtain good physical and chemical properties of the product requires specific lighting parameters, but the rate of post-curing parameters corresponding to excellent physical and chemical properties is usually very fast, which means that a lot of heat will be generated in a short time. This phenomenon is caused by the following reasons:

[0004] Light energy is converted into heat energy: Ultraviolet light (UV light) is a high-energy electromagnetic wave. When UV light is irradiated onto photosensitive materials (such as photosensitive resin), these materials absorb the light energy and part of the light energy is converted into heat energy, resulting in an increase in temperature;

[0005] Photochemical reaction releases heat: Under the irradiation of ultraviolet light, photochemical reactions such as free radical polymerization or cationic polymerization occur inside the photosensitive material. These reactions break the chemical bonds of the molecules and form new bonds. In this process, part of the chemical energy is released in the form of heat energy;

[0006] Internal friction of materials: Under the irradiation of ultraviolet light, the molecules inside the material are rearranged and cross-linked, which causes friction between molecules and generates heat. This molecular movement and friction also causes the temperature to rise;

[0007] The role of photosensitizers and photoinitiators: photosensitizers and initiators will decompose into free radicals or other active species under the action of ultraviolet light, which will trigger polymerization reactions to form long-chain polymers. In this process, part of the energy will be released in the form of heat.

[0008] During the curing process of composite materials, the thickness of the shell-like product affects the uniformity of its internal temperature, resulting in differences in the degree of curing in the time domain and space domain and generating internal residual stress. This heat can neither be promptly discharged through the thermal base nor instantaneously regulated by the ambient temperature, so it will accumulate on the product. However, once this heat cannot be dissipated in a timely and effective manner, a temperature gradient will be generated in the local area, resulting in uneven expansion or contraction of the material. This uneven expansion can further aggravate the internal stress, thereby causing deformation or loss of precision of the final product. Moreover, after being heated, the color of the orthodontic appliance will easily turn white, affecting subsequent medical observations.

[0009] When the post-curing process is carried out at low temperature, the temperature also has an impact on the post-curing process. For example, the temperature not only affects the rate of polymerization, but also affects the physical properties of the material and the final cured state. Specifically, at ultra-low temperatures, the rate of polymerization slows down significantly. This is because the molecular motion slows down and the collision opportunities between reactants decrease, resulting in a decrease in the reaction rate. The material in this state may not be easy to move the molecules in the polymerization reaction, thereby affecting the cross-linking density and the final performance of the material.

[0010] Therefore, a method is needed to solve the above problems. Summary of the invention

[0011] Therefore, in order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a post-curing method for a 3D thin-walled shell product, which can control the reaction temperature of the product in the entire post-curing process within a preset range and quickly take away the heat generated by the violent reaction, thereby minimizing deformation while ensuring the physical properties of the product.

[0012] In order to achieve the above-mentioned purpose, the present invention provides a post-curing method for a 3D thin-walled shell-like product, comprising: continuously spraying the surface of a thin-walled shell-like product that has been 3D printed with a plasma gas flow at 8°C to 12°C, wherein the proportion of nitrogen in the plasma gas flow is not less than 95% and the oxygen content is not more than 2%; the maximum thickness of the thin-walled shell-like product is between 0.2mm and 2.0mm; post-curing the thin-walled shell-like product in a photo-induced manner by ultraviolet light, the reaction temperature of the entire post-curing process is in the range of 0°C to 20°C, and the plasma gas flow is maintained at a predetermined speed during the post-curing process; after the post-curing is completed, turning off the ultraviolet lamp, then turning off the plasma equipment, and taking out the thin-walled shell-like product.

[0013] In one embodiment, the plasma gas flow is a combined flow of nitrogen and an inert gas.

[0014] In one embodiment, the distance between the nozzle ejecting the plasma gas flow and the thin-walled shell-shaped product is between 15 and 25 mm.

[0015] In one embodiment, after the surface of the 3D printed thin-walled shell-like product is continuously sprayed with plasma airflow for a predetermined period of time, the thin-walled shell-like product is post-cured by ultraviolet light.

[0016] In one embodiment, the predetermined time is 10s to 60min.

[0017] In one embodiment, the power of the plasma gas flow ranges from 60W to 100W.

[0018] In one embodiment, the thin-walled shell product is post-cured by ultraviolet light using a specific illumination interval.

[0019] In one embodiment, the reaction temperature of the entire post-curing process is in the range of 7°C to 17°C.

[0020] In one embodiment, the thin-walled shell-shaped product is placed on a metal mesh in the post-curing box, and the mesh gap of the metal mesh is 2mm×2mm to 20mm×20mm.

[0021] In one embodiment, the wavelength range of the ultraviolet light is 410-315 nm.

[0022] In one embodiment, the predetermined velocity of the plasma gas flow at the nozzle is 60-100 m / s.

[0023] In one embodiment, the thin-walled shell product may be an appliance.

[0024] Compared with the prior art, the advantages of the present invention are: using plasma gas flow to "burn" uncured monomers or polymers on the surface of the object through various mechanisms, and using the low temperature of the plasma gas flow itself to form heat convection to take away the heat generated by the polymerization reaction triggered by ultraviolet light, so that no temperature gradient is generated inside the thin-walled shell-like product, thereby ensuring uniform expansion or contraction of the thin-walled shell-like product, avoiding deformation of the thin-walled shell-like product, and ensuring the accuracy of the final thin-walled shell-like product. The low temperature of the plasma gas flow itself can also prevent the thin-walled shell-like product from turning white due to heat, ensuring the transparency of the final product, which is beneficial to the invisible effect / aesthetics of subsequent products. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0026] Figure 1is a schematic flow chart of a post-curing method for a 3D thin-walled shell-shaped product in an embodiment of the present invention;

[0027] Figure 2 It is a process of post-curing the 3D thin-walled shell-shaped product in the embodiment of the present invention in a post-curing box;

[0028] Figure 3 is a graph of stress relaxation performance of a 3D thin-walled shell-shaped product measured under different post-curing conditions in an embodiment of the present invention;

[0029] Figure 4 It is a scatter plot of elastic modulus and global dimensional deviation of a 3D thin-walled shell product in an embodiment of the present invention. DETAILED DESCRIPTION

[0030] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0031] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0032] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0033] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0034] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0035] Before the 3D printing and post-curing process of thin-walled shell products, residual photoinitiators remain in the matrix material and cannot be easily removed. In general product material properties, the glass transition temperature (Tg) is between 40°C and 220°C, so the post-curing temperature needs to be controlled to avoid deformation of the final product.

[0036] like Figure 1 As shown, the embodiment of the present application provides a post-curing method for a 3D thin-walled shell-shaped product, comprising the following steps:

[0037] S1, using a plasma gas flow at 8°C to 12°C to continuously spray the surface of the thin-walled shell-shaped product that has been 3D printed for a predetermined time, and the proportion of nitrogen in the plasma gas flow is not less than 95%.

[0038] In the plasma gas flow, the proportion of nitrogen (N2) should be above 95%. Plasmas generated by different gases in the plasma gas flow have different chemical activities, which will affect their chemical reaction ability with monomers or polymers in the 3D printing substrate system. Therefore, the gas ratio in the plasma gas flow can be adjusted as needed to ensure the subsequent "combustion" result. In this embodiment, the plasma gas flow does not contain oxygen (O2).

[0039] Thin-walled shell products are placed in Figure 2 At a predetermined position in the post-curing box shown. The surface of the thin-walled shell-like product that has been 3D printed is continuously sprayed with a plasma gas flow of 8°C to 12°C. The purpose of the continuous spraying is to ensure that the surface reacts fully during UV curing. In one embodiment, the thin-walled shell-like product can be an orthodontic appliance.

[0040] S2, post-curing the thin-walled shell product by ultraviolet light in a photo-initiated manner, the reaction temperature of the entire post-curing process is in the range of 0°C to 20°C, and the plasma gas flow is maintained at a predetermined speed during the post-curing process.

[0041] The ultraviolet light can be provided by the ultraviolet lamp on the top surface of the post-curing box. The wavelength of the ultraviolet light can range from 200 to 410 nm. The reaction temperature of the entire post-curing process is in the range of 0°C to 20°C, and during the post-curing process, the plasma gas flow continues to spray on the thin-walled shell product.

[0042] In this embodiment, the mechanism of removing uncured monomers or polymers on the surface of the product by the plasma gas flow mainly involves the chemical and physical effects of the plasma, as well as some other effects, specifically including:

[0043] a. Chemical action: Plasma contains highly active particles, such as free radicals, excited atoms and molecules, and ions, etc. These particles can react chemically with uncured monomers or polymers on the surface of objects, causing them to decompose or transform into small molecules that are easily volatile or easily removed, thereby achieving a "burning" effect.

[0044] b. Physical effect: High-energy particles of plasma (such as electrons) can directly bombard the surface of an object and remove unsolidified materials by physical stripping.

[0045] c. Thermal effects: Although non-high temperature plasma is used, the plasma still produces local thermal effects when interacting with the surface of an object, which may help promote chemical reactions or change the physical state of the substance, making it easier to remove.

[0046] d. Ultraviolet radiation: Some particles in the plasma will emit ultraviolet light when returning to the ground state. This radiation can destroy the chemical bonds of the material and help decompose uncured monomers or polymers.

[0047] These mechanisms work together to effectively remove uncured monomers or polymers from the surface of an object. It should be noted that "combustion" here does not mean the traditional combustion reaction (i.e., reaction with oxygen to produce flames and heat), but refers to the process of efficiently removing and converting uncured materials achieved through plasma treatment technology.

[0048] S3, after the post-curing is completed, turn off the UV lamp, then turn off the plasma equipment, and take out the thin-walled shell product.

[0049] Steps S1 and S2 can be performed almost simultaneously, or step S1 can be performed first and then step S2. As long as the thin-walled shell-like product is kept in the plasma airflow during the post-curing process of the thin-walled shell-like product being irradiated with ultraviolet light, the thin-walled shell-like product can be placed in a closed post-curing box for post-curing, or it can be maintained in the plasma airflow by other facilities.

[0050] The above method uses plasma gas flow to "burn" uncured monomers or polymers on the surface of the object through various mechanisms, and uses the low temperature of the plasma gas flow itself to form thermal convection to remove the heat generated by the polymerization reaction triggered by ultraviolet light, so that no temperature gradient is generated inside the thin-walled shell-like product, thereby ensuring uniform expansion or contraction of the thin-walled shell-like product, avoiding deformation of the orthodontic appliance, and ensuring the accuracy of the final orthodontic appliance. The low temperature of the plasma gas flow itself can also prevent the orthodontic appliance from turning white due to heat, ensuring the transparency of the final product, which is conducive to subsequent medical observation.

[0051] In one embodiment, the plasma gas flow is a combined flow of nitrogen and an inert gas.

[0052] The plasma gas flow is nitrogen or a combination of nitrogen and inert gas. Inert gas refers to gaseous single substances or their combinations corresponding to all Group 0 elements on the periodic table. For example, the gaseous single substances may be helium (He), neon (Ne), argon (Ar), krypton (Kr), xenon (Xe), radon (Rn), Gas (Og), etc.

[0053] The distance between the plasma and the material surface also affects the treatment effect. If the distance is too far, the active particles of the plasma may lose their activity before reaching the material surface, while if the distance is too close, the material may be overheated or damaged. In one embodiment, the distance between the nozzle that ejects the plasma gas flow and the thin-walled shell product is between 15 and 25 mm.

[0054] In one embodiment, after the surface of the 3D printed thin-walled shell-like product is continuously sprayed with plasma airflow for a predetermined period of time, the thin-walled shell-like product is post-cured by ultraviolet light.

[0055] In one embodiment, the predetermined time of spraying is 10 seconds to 60 minutes.

[0056] The calculation of plasma machine power is related to the characteristics and operating parameters of the plasma. First, the power density of the plasma is an important parameter for measuring the power of the ion beam. Power density is defined as the power per unit area. During the plasma generation process, the gas is heated and ionized to form a plasma. The power density calculation formula is power density = power / area. In one embodiment, the power range of the plasma gas flow is 60 to 100W. The fixed light wavelength is 405nm, from Figure 3 As can be seen from the experimental results, the generation and maintenance of plasma requires a certain amount of power, and the power level will affect the density and temperature of the plasma, and further affect the rate and efficiency of the chemical reaction. Preferably, the power range of the plasma gas flow is 60 to 100W.

[0057] In one embodiment, the predetermined velocity of the plasma gas flow at the nozzle is 60-100 m / s. The predetermined velocity cannot be too high to avoid blowing away the thin-walled shell-shaped product, nor can it be too low to effectively cool down the product.

[0058] In one embodiment, the thin-walled shell product is post-cured by ultraviolet light using a specific exposure interval.

[0059] Taking the stress relaxation performance of the material as an example, a standard dumbbell-shaped specimen was made and stretched for 24 hours at 3% strain. The ratio of the final force value to the initial force value was recorded, which is the residual ratio of stress relaxation. Figure 3 The experimental results show that under different plasma gas flow powers and different illumination intervals, the stress relaxation properties of the obtained materials are significantly different. The illumination interval is generally within 1s to 5min.

[0060] In one embodiment, the reaction temperature of the entire post-curing process is in the range of 7° C. to 17° C. When the post-curing light parameter is fixed at 40 mW / cm 2 When there is no interval exposure, different reaction temperatures will affect some physical properties of the material (such as elastic modulus) and the accuracy of the product (such as global dimensional deviation). When it is necessary to obtain an elastic modulus as close to 2000Mpa as possible and a product dimensional deviation as small as possible, the test data such as Figure 4 Therefore, it is actually necessary to control the reaction temperature of the product post-curing at least between 0°C and 20°C, preferably within the range of 12°C±5°C.

[0061] In one embodiment, the thin-walled shell-shaped product is placed on a metal mesh in a post-curing box, and the mesh gap of the metal mesh is 2mm×2mm to 20mm×20mm.

[0062] In one embodiment, the wavelength of the ultraviolet light is in the range of 515 to 315 nm. The longer the wavelength of the ultraviolet light is, the easier it is for it to penetrate the product, thereby ensuring that the thin-walled shell product is cured both inside and outside at the same time.

[0063] Embodiment 1

[0064] The thin-walled shell product can be an orthodontic appliance that uses DLP technology to directly 3D print a polyurethane (PUA) substrate system. Such a substrate system includes pre-polymerized polyurethane, (meth) acrylate monomers (Acrylate Monomers) with one or more single functional groups, diluents, photoinitiators, and other additives.

[0065] The polyurethane matrix (PUA) is prepolymerized polyurethane, accounting for 20% to 50% by weight of the total formula. PUA with moderate molecular weight, good biocompatibility and appropriate mechanical strength is selected, specifically, the molecular weight of PUA is within 3500-22000Da.

[0066] The (meth)acrylate monomers (Acrylate Monomers) may be methyl methacrylate (MMA), 1,6-hexanediol diacrylate (HDDA), trimethylolpropane triacrylate (TMPTA), etc. The weight ratio of the (meth)acrylate monomers (Acrylate Monomers) accounts for 25% to 85% of the total formula.

[0067] The diluent is used to adjust the viscosity of the substrate to ensure good printing fluidity. The diluent can be ethyl acetate. The weight ratio of the diluent accounts for 5% of the total formula.

[0068] The photoinitiator is used to ensure an effective photocuring reaction. The photoinitiator may be 2-hydroxy-2-methylpropionate (HMPP), accounting for 5% of the total formulation.

[0069] Other additives: including UV blockers, inhibitors and antioxidants, etc. The weight of the total formula is not more than 5%.

[0070] 3D printing parameters: The illumination time is set to 10-15 seconds per layer, and the illumination intensity is adjusted to 1-5mW / cm 2 , so that the PUA is cured and formed, but the resin containing the photoinitiator remains on the surface.

[0071] Printing process: Printing is done using a DLP 3D printer, and the support height is raised after each layer is printed to form the next layer.

[0072] The surface of the 3D printed thin-walled shell-shaped product in the post-curing box is continuously sprayed with a plasma gas flow at 8°C to 12°C for a predetermined time (3 minutes), and the proportion of nitrogen in the plasma gas flow is not less than 95%; the power of the plasma gas flow adopts a rated power of 80W;

[0073] The thin-walled shell product is post-cured by ultraviolet light in a photo-initiated manner. The reaction temperature of the entire post-curing process (5 minutes) is in the range of 0°C to 20°C. The plasma gas flow is maintained at a predetermined speed (80m / s) during the post-curing process.

[0074] After the post-curing is completed, turn off the UV lamp, then turn off the plasma equipment, and take out the thin-walled shell product.

[0075] After the above-mentioned post-curing process, the elastic modulus of the appliance was measured to be 1432 MPa, the dimensional deviation was the maximum deformation in the arch width direction of 0.6 mm, the haze was 3.2%, and the projection rate was 88%.

[0076] Embodiment 2

[0077] Thin-walled shell products can be directly 3D printed using SLA technology. Silicone-based systems. Such substrate systems include monomers or oligomers of dimethacrylate based on silicon or silicon polyurethane, one or more monomers / oligomers of cyclic (meth)acrylates, polycarbonate diols, photoinitiators, and aliphatic or cycloaliphatic dimethacrylates.

[0078] Wherein, 15-85% by weight of monomer or oligomer dimethacrylate based on silicon or silicon polyurethane, with a viscosity of <100 Pa·s, may specifically include:

[0079] 1) Multifunctional silicone acrylate, 20-40% by weight;

[0080] 2) 3-methacryloxypropyltrimethoxysilane (MAPTMS), 5-10% by weight;

[0081] 3) Methacrylate-terminated Silicone Polyurethane, 30-60% by weight;

[0082] 4) Acrylate-functionalized Siloxane-Polyurethane Copolymers, 20-55% by weight.

[0083] 20-50% by weight of one or more monomeric / oligomeric cyclic (meth)acrylates with a viscosity of <0.5 Pa·s.

[0084] 1-25% by weight of polycarbonate diol, the viscosity of the polycarbonate diol is less than 10 Pa·s.

[0085] 0.1-5% by weight of a photoinitiator, the photoinitiator may have one or more absorption wavelength ranges of a laser beam or radiation source.

[0086] 2-20% by weight of aliphatic or cycloaliphatic dimethacrylate, the viscosity of the aliphatic or cycloaliphatic dimethacrylate is less than 10 Pa·s.

[0087] 3D printing parameters: The illumination time is set to 10-15 seconds per layer, and the illumination intensity is adjusted to 1-5mW / cm 2, so that the PUA is cured and formed, but the resin containing the photoinitiator remains on the surface.

[0088] Printing process: Printing is done using a DLP 3D printer, and the support height is raised after each layer is printed to form the next layer.

[0089] The surface of the 3D printed thin-walled shell-shaped product in the post-curing box is continuously sprayed with a plasma gas flow at 8°C to 12°C for a predetermined time (15s), and the proportion of nitrogen in the plasma gas flow is not less than 95%; the power of the plasma gas flow adopts a rated power of 65W;

[0090] The thin-walled shell product is post-cured by ultraviolet light in a photo-initiated manner. The reaction temperature of the entire post-curing process (5 minutes) is in the range of 0°C to 20°C. The plasma gas flow is maintained at a predetermined speed (70m / s) during the post-curing process.

[0091] After the post-curing is completed, turn off the UV lamp, then turn off the plasma equipment, and take out the thin-walled shell product.

[0092] After the above post-curing process, the elastic modulus of the product was measured to be 983 MPa, the dimensional deviation was a maximum deformation of 1.3 mm in the bow width direction, the haze was 6.8%, and the projection rate was 76%.

[0093] Embodiment 3

[0094] Thin-walled shell products can be directly 3D printed using DLP technology on the PUA substrate system.

[0095] The PUA material system includes:

[0096] 15 to 95% by weight of a monofunctional polyurethane methacrylate oligomer having at least one polymerizable group and a number average molecular weight (Mn) of 35 to 14500 g / mol;

[0097] 30-60 wt % of a reactable compound comprising at least one of an acrylate monomer or oligomer, a methacrylate monomer or oligomer, a vinyl ester monomer or oligomer, and an acrylamide monomer or oligomer;

[0098] No greater than 10% of at least one diluent compound having at least one ethylenically unsaturated functional group;

[0099] No more than 5% of at least one photoinitiator;

[0100] The composition has a viscosity of 1 to 70 Pa·s at 40° C. and a Tg of 40° C. or higher.

[0101] 3D printing parameters: The illumination time is set to 10-15 seconds per layer, and the illumination intensity is adjusted to 1-5mW / cm 2 , so that the PUA is cured and formed, but the resin containing the photoinitiator remains on the surface.

[0102] Printing process: Printing is done using a DLP 3D printer, and the support height is raised after each layer is printed to form the next layer.

[0103] The surface of the 3D printed thin-walled shell-shaped product in the post-curing box is continuously sprayed with a plasma gas flow at 8°C to 12°C for a predetermined time (1s), and the proportion of nitrogen in the plasma gas flow is not less than 95%; the power of the plasma gas flow adopts a rated power of 90W;

[0104] The thin-walled shell product is post-cured by ultraviolet light in a photo-initiated manner. The reaction temperature of the entire post-curing process (10 minutes) is within the range of 0°C to 20°C. The plasma gas flow is maintained at a predetermined speed (60m / s) during the post-curing process.

[0105] After the post-curing is completed, turn off the UV lamp, then turn off the plasma equipment, and take out the thin-walled shell product.

[0106] After the above post-curing process, the elastic modulus of the product was measured to be 1603MPa, the dimensional deviation was the maximum deformation in the bow width direction was 0.3mm, the haze was 1.3%, and the projection rate was 91%.

[0107] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A post-curing method for 3D printed thin-walled shell products, characterized in that: include: The surface of the 3D printed thin-walled shell-like product is continuously sprayed with a plasma gas flow at 8°C to 12°C, wherein the proportion of nitrogen in the plasma gas flow is not less than 95% and the proportion of oxygen is not more than 2%; the maximum thickness of the thin-walled shell-like product is between 0.2mm and 2.0mm; Post-curing the thin-walled shell product by ultraviolet light in a photo-induced manner, wherein the reaction temperature of the entire post-curing process is within a range of 0° C. to 20° C., and the plasma gas flow is maintained at a predetermined speed during the post-curing process; After the post-curing is completed, turn off the UV lamp, then turn off the plasma equipment, and take out the thin-walled shell product.

2. The post-curing method according to claim 1, characterized in that: The plasma gas flow is a combined gas flow of nitrogen and inert gas.

3. The post-curing method according to claim 1, characterized in that: The distance between the nozzle for ejecting the plasma gas flow and the thin-walled shell-shaped product is between 15 and 25 mm.

4. The post-curing method according to claim 1, characterized in that: After the surface of the 3D printed thin-walled shell-like product is continuously sprayed with plasma airflow for a predetermined period of time, the thin-walled shell-like product is post-cured by ultraviolet light.

5. The post-curing method according to claim 4, characterized in that: The predetermined time is 10s to 60min.

6. The post-curing method according to claim 1, characterized in that: The power range of the plasma gas flow is 60-100W.

7. The post-curing method according to claim 1, characterized in that: The thin-walled shell product is post-cured by ultraviolet light using a specific illumination interval.

8. The post-curing method according to claim 1, characterized in that: The reaction temperature of the entire post-curing process is in the range of 7°C to 17°C.

9. The post-curing method according to claim 1, characterized in that: The thin-walled shell-shaped product is placed on a metal mesh in the post-curing box, wherein the mesh gap of the metal mesh is 2 mm×2 mm to 20 mm×20 mm.

10. The post-curing method according to claim 1, characterized in that: The wavelength range of the ultraviolet light is 515-315 nm.

11. The post-curing method according to claim 1, characterized in that: The predetermined velocity of the plasma gas flow at the nozzle is 60-100 m / s.

12. The post-curing method according to claim 1, characterized in that: The thin-walled shell-shaped product is an orthodontic appliance.

Citation Information

Patent Citations

  • Flexible pressure sensor chip based on 3D printing technology and production method thereof

    CN108515694A

  • Post-curing method and device of fiber reinforced thermosetting composite 3D printing component

    CN109203464A

  • Preparation method of novel photoetching diaphragm plate

    CN116626986A

  • Feature forming process using plasma treatment

    EP2228156A1

  • High temperature three dimensional printing compositions

    US20160369040A1