Interlayer toughening fiber composite material as well as preparation method and application thereof

By spraying micro- and nano-sized toughened particles into the fiber composite, interlayer toughened fiber composite materials are formed, which solves the problem of layering failure of thermosetting resin-based materials under load, improves interlayer fracture toughness and reduces Production cost, suitable for high-end applications.

CN118906492APending Publication Date: 2024-11-08NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411359435.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Thermoset resin-based fiber composites are prone to stratification damage under loads such as in-plane compression, bending, fatigue and lateral impact, resulting in failure and limiting their application.

Method used

Spraying technology is used to disperse micro- and nano-sized toughened particles in low viscosity and volatile solvents to form mixed toughened particles dispersion liquid, applied to fiber cloth or prepreg, composite with resin and cure, forming inter-layer enhancement Tough fiber composite material.

Benefits of technology

Through multi-step gradient interface and multi-scale toughening effect, the interlayer fracture toughness of composite materials is significantly improved, the production cost is reduced, and the original molding process is maintained. It is suitable for automobiles, aerospace and ships.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906492A_ABST
    Figure CN118906492A_ABST
Patent Text Reader

Abstract

The invention discloses an interlayer toughening fiber composite material as well as a preparation method and application thereof. The preparation method comprises the following steps: dispersing micron-scale toughening particles and nano-scale toughening particles in a solvent to form a mixed toughening particle dispersion liquid; wherein the solvent is a low-viscosity and volatile solvent; and the mixed toughening particle dispersion liquid is applied to fiber cloth in a spraying mode, then the fiber cloth is compounded with resin, curing forming is conducted, and the interlayer toughening fiber composite material is prepared, or applying the mixed toughening particle dispersion liquid to the prepreg in a spraying manner, and then performing curing molding to obtain the interlayer toughening fiber composite material. According to the present invention, the permeability of the micron-scale toughening particles, the nano-scale toughening particles and the resin is different, such that the multi-scale gradient interface is formed between the fiber layers so as to achieve the multi-scale toughening, and the dispersion process provided by the present invention is simple, does not change the original molding process of the fiber composite material, and is suitable for industrial production; good application prospects are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to an interlayer toughened fiber composite material and a preparation method and application thereof. Background Art

[0002] Fiber-reinforced resin-based composites (FRP) can comprehensively play the advantages of two components and are widely used in many fields such as automobiles, aerospace, ships, sports, etc. Among them, fiber composites based on thermosetting resins such as epoxy resins, bismaleimide resins, polyimide resins, etc. are increasingly used in high-end fields. However, thermosetting resins are brittle and have low toughness. At the same time, they are limited by the layered structure characteristics of FRP composites, which makes them prone to delamination under loads such as in-plane compression, bending, fatigue and lateral impact, leading to catastrophic failure and limiting their application. Therefore, improving the interlaminar fracture toughness of FRP composites is crucial in many engineering applications.

[0003] At present, the main toughening modification methods include resin toughening, Z-direction toughening and interlayer toughening. Among them, interlayer toughening refers to the toughening of composite materials by introducing toughening materials such as particles, fibers, and films between the layers of composite materials. This method does not change the original molding process of fiber composite materials, and the toughening materials directly act on the weak layers of the composite materials, with less weakening of the in-plane mechanical properties. Among them, introducing toughening particles into CFRP composites through spraying technology can improve the fracture toughness and overall damage perception ability of composite laminates, which has received widespread attention in recent years. Summary of the invention

[0004] The main purpose of the present invention is to provide an interlayer toughened fiber composite material and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: An embodiment of the present invention provides a method for preparing an interlayer toughened fiber composite material, which comprises: Dispersing micron-sized toughening particles and nano-sized toughening particles in a solvent to form a mixed toughening particle dispersion; wherein the solvent is a low-viscosity, volatile solvent; Also, the mixed toughening particle dispersion is applied to the fiber cloth by spraying, and then compounded with resin and cured to obtain an interlayer toughening fiber composite material; or, the mixed toughening particle dispersion is applied to the prepreg by spraying, and then cured to obtain an interlayer toughening fiber composite material.

[0006] The embodiment of the present invention also provides an interlaminar toughening fiber composite material obtained by the aforementioned preparation method.

[0007] The embodiment of the present invention also provides the use of the above-mentioned interlaminar toughened fiber composite material in the fields of automobiles, aerospace or ships.

[0008] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention provides a simple, industrially applicable method for toughening the interlayers of fiber composite materials; on the one hand, due to the different out-of-plane mobility (permeability) of micron-sized particles, nano-sized particles and resins, a multi-order gradient interface is formed between the fiber layers, and multi-scale toughening is performed to achieve a better toughening effect (compared with the interlayer toughening of micron-sized or nano-sized particles alone); on the other hand, micron-sized particle aramid pulp is used to replace part of the nano-sized particle carbon nanotubes, which can greatly reduce the production cost while achieving efficient toughening and has a large application scenario. In addition, the present invention uses a relatively simple dispersion process, and the processing method of the fiber cloth / prepreg does not change the original molding process of the fiber composite material, and is easy to further promote and apply. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0010] Figure 1 is a process flow chart of a high pressure spraying technology in a typical embodiment of the present invention; Figure 2a-2b is a SEM photograph of the micron-sized aramid pulp particles and the nano-sized carbon nanotube particles in Example 1 of the present invention; Figure 3a-3d is a surface SEM photograph of toughened particle-modified glass fibers of different scale structures in Example 1 of the present invention; Figure 4a-4d is a surface microscope image of toughened particle-modified glass fiber of different scale structures in Example 1 of the present invention; Figure 5 1 is a graph showing the test results of the double cantilever beam of Example 1 of the present invention and Comparative Example 1; Figure 6 : is an R curve diagram (a curve of crack propagation resistance versus crack propagation) of the double cantilever beam of Example 1 of the present invention and Comparative Example 1; Figure 7 1 is a graph showing the end delamination flexure (ENF) test results of Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0011] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0012] Specifically, as one aspect of the technical solution of the present invention, a method for preparing an interlayer toughened fiber composite material includes: Dispersing micron-sized toughening particles and nano-sized toughening particles in a solvent to form a mixed toughening particle dispersion; wherein the solvent is a low-viscosity, volatile solvent; Also, the mixed toughening particle dispersion is applied to the fiber cloth by spraying, and then compounded with resin and cured to obtain an interlayer toughening fiber composite material; or, the mixed toughening particle dispersion is applied to the prepreg by spraying, and then cured to obtain an interlayer toughening fiber composite material.

[0013] In some preferred embodiments, the micron-sized toughening particles include micron-sized aramid pulp, but are not limited thereto.

[0014] Furthermore, the micron-sized aramid pulp includes interfacially modified aramid pulp and / or non-interfacially modified aramid pulp.

[0015] In some preferred embodiments, the particle size of the micron-sized toughening particles is 50-200 μm.

[0016] In some preferred embodiments, the nanoscale toughening particles include carbon nanotubes, but are not limited thereto.

[0017] Furthermore, the carbon nanotubes include surface-modified carbon nanotubes and / or non-surface-modified carbon nanotubes.

[0018] Furthermore, the carbon nanotubes include carbon nanotubes with functional groups grafted on the surface, wherein the functional groups include any one or more combinations of carboxyl groups, amino groups, and hydroxyl groups, but are not limited thereto.

[0019] In some preferred embodiments, the particle size of the nanoscale toughening particles is 10-50 nm.

[0020] In some preferred embodiments, the solvent includes any one or more combinations of water, alcohol, and acetone, but is not limited thereto.

[0021] In some preferred embodiments, the usage ratio of the micron-sized toughening particles and nano-sized toughening particles to the solvent is 0.01-0.03 g: 0.01-0.03 g: 100 ml.

[0022] Furthermore, the usage ratio of the micron-scale toughening particles, nano-scale toughening particles and the solvent is 0.02g:0.02g:100ml.

[0023] In some preferred embodiments, the preparation method specifically comprises: Using a high-pressure spray gun device to evenly spray the mixed toughening particle dispersion on the fiber cloth, and wait for the solvent to evaporate and remove, so as to obtain a modified fiber cloth; stacking and arranging a plurality of modified fiber cloths to form a fiber preform; Furthermore, the resin and the curing agent are mixed to form a resin-based slurry, and the resin-based slurry is then introduced into a fiber preform, and then cured and formed to obtain an interlayer toughened fiber composite material.

[0024] Furthermore, the fiber cloth includes any one or more combinations of carbon fiber cloth, glass fiber cloth, basalt cloth, and aramid fiber cloth, but is not limited thereto.

[0025] Furthermore, the fiber cloth includes any one of unidirectional fiber cloth, bidirectional fiber cloth, and three-dimensional fiber cloth, but is not limited thereto.

[0026] Further, the resin includes any one or more combinations of epoxy resin, polyester, phenolic resin, vinyl ester, bismaleimide, and thermoplastic resin, but is not limited thereto.

[0027] In some preferred embodiments, the preparation method specifically comprises: Using a high-pressure spray gun device to evenly spray the mixed toughening particle dispersion on the prepreg, and wait for the solvent to evaporate and remove, so as to obtain a modified prepreg; Furthermore, a plurality of modified prepregs are stacked and arranged, and then cured and formed to obtain an interlayer toughened fiber composite material.

[0028] Further, the prepreg includes bismaleimide resin / carbon fiber prepreg and / or epoxy resin / carbon fiber prepreg, but is not limited thereto.

[0029] In some preferred embodiments, the curing molding includes any one of VARTM, RTM, hand lay-up molding, compression molding, and autoclave molding, but is not limited thereto.

[0030] In the present invention, the aramid pulp / carbon nanotube mixed particles (micron-sized aramid pulp particles and nano-sized carbon nanotube particles) form a multi-scale structure of micron and nanometer levels. The mixed particles with the multi-scale structure are evenly dispersed in a low-viscosity, volatile dispersant solution, and the solution containing the mixed particles is evenly sprayed on the fiber cloth / prepreg by a high-pressure spray gun. After the solvent on the fiber cloth / prepreg is removed, the modified fiber cloth is composited with the resin; the modified prepreg is directly processed and formed. The process flow chart of the high-pressure spraying technology is shown in the figure. Figure 1 shown.

[0031] Preferably, the micron-sized particle aramid pulp is interfacially modified or not interfacially modified.

[0032] Preferably, the surface of the nano-sized particle carbon nanotube is modified or unmodified.

[0033] Preferably, the surface of the nano-sized carbon nanotube particles is grafted with functional groups, and the functional groups include any one of carboxyl, amino or hydroxyl groups or a combination of two or more thereof.

[0034] Preferably, the low-viscosity, volatile dispersant solution includes but is not limited to water, alcohol, acetone, etc.

[0035] Preferably, the fiber cloth includes but is not limited to carbon fiber, glass fiber, basalt or aramid fiber, etc.

[0036] Preferably, the fiber cloth structure includes but is not limited to unidirectional, bidirectional and three-dimensional structures.

[0037] Preferably, the resin includes but is not limited to epoxy resin, polyester, phenolic resin, vinyl ester, bismaleimide, etc. and thermoplastic resin.

[0038] Preferably, the prepreg includes but is not limited to bismaleimide resin / carbon fiber prepreg, epoxy resin / carbon fiber prepreg and the like.

[0039] Preferably, the molding process includes but is not limited to VARTM, RTM, hand lay-up molding, compression molding, autoclave molding, etc.

[0040] In some more specific embodiments, the method for preparing the interlayer toughened fiber composite material comprises the following steps: (1) Mixing micron-sized aramid pulp particles and nano-sized carbon nanotube particles in a certain mass ratio to obtain mixed toughening particles with a multi-scale structure, and then dispersing them in a low-viscosity, volatile dispersant solution (such as ethanol or acetone). The dispersion method includes but is not limited to ultrasound, ball milling, grinding, mechanical stirring, microfluidics, etc. The process requires step-by-step dispersion from coarse to fine to achieve the best dispersion effect; (2) spraying the dispersant solution containing toughening particles uniformly onto the fiber cloth / prepreg by a high-pressure spray gun, and then transferring the fiber cloth / prepreg into a vacuum oven to remove the residual solvent; (3) Use standard molding processes such as VARTM, RTM, hand lay-up, autoclave, etc.

[0041] Another aspect of the embodiments of the present invention further provides an interlaminar toughened fiber composite material obtained by the aforementioned preparation method.

[0042] Another aspect of the embodiments of the present invention further provides use of the aforementioned interlaminar toughened fiber composite material in the fields of automobiles, aerospace or ships.

[0043] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0044] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0045] Example 1 This embodiment illustrates the preparation process of the aramid pulp / carbon nanotube mixed interlayer toughening fiber composite material, which is specifically as follows: S1. Uniformly disperse the multi-scale structured mixed toughening particles in acetone solution Weigh 0.0188 g of micron-sized toughening aramid powder and nano-sized toughening carbon nanotube (CNT) particles, respectively, add them into a certain amount of acetone, stir evenly with a glass rod, and treat them with an ultrasonic cell disruptor at room temperature (25°C) for 10 min to make the mixed micro-nano toughening particles disperse relatively evenly, and obtain a preliminarily dispersed mixed toughening particle acetone solution; SEM photos of micron-sized aramid pulp particles and nano-sized carbon nanotube particles in this embodiment are shown in FIG. Figure 2a-2b ; S2. Spraying the acetone solution containing mixed micro-nano toughening particles onto the glass fiber fabric Take the glass fiber bidirectional cloth and cut a piece of 25 × 50 cm 2The glass fiber fabric is poured into a high-atomization spray gun, and the spray gun is connected to an air compressor (it is recommended to be equipped with an air purifier) ​​or a nitrogen bottle. The spraying pressure is 0.40 MPa, and the spraying distance is 30 cm. The mixed micro-nano toughening particle acetone solution is evenly sprayed on the glass fiber fabric. Then, a breathable cloth is covered, and the acetone is evaporated and dried to prepare a glass fiber fabric containing 0.3 gsm of mixed micro-nano toughening particles; S3. Preparation of fiber preform Take the glass fiber bidirectional cloth and cut it into 25×25 cm 2 The fiber preform is then laid by hand-stacked method. Specifically, 20 layers of glass fiber bidirectional cloth are stacked and arranged, of which 10 layers and 11 layers of fiber cloth are coated with mixed micro-nano toughening particle coating on one side and arranged oppositely, and a 45 mm long polytetrafluoroethylene film (30 μm thick) is laid as a pre-crack; S4. Preparation of composite material board The composite material board is prepared by the VARTM method. Specifically, a double-layer guide net is used for the laid fiber preform, and the guide net and the fiber preform are separated by a release cloth, and finally sealed with a vacuum bag.

[0046] Prepare epoxy resin-based slurry: pour 300g of bisphenol F epoxy resin Epon862 into a beaker, then add 105.6g of curing agent D-230, and stir thoroughly with a mixing and degassing machine to obtain about 405.6g of resin-based slurry.

[0047] The resin-based slurry is uniformly introduced into the fiber preform through the negative pressure of the vacuum pump. After the resin-based slurry is completely infused into the carbon fiber cloth, the VARTM platform is moved as a whole into the flat vulcanizer, first cured at 80 °C and 1 MPa pressure for 2 h, and then cured at 120 °C for 2 h. After that, it is cooled and demoulded to obtain a composite material plate.

[0048] The surface SEM photos of the toughened particles modified glass fibers of different scale structures in this embodiment are shown in FIG. Figure 3a-3d As shown; the surface microscope images of toughened particles modified glass fibers with different scale structures are shown in Figure 4a-4d shown.

[0049] Comparative Example 1 In this comparative example 1, no toughening particle component is introduced, and the remaining steps and parameters are the same as those in Example 1.

[0050] Comparative Example 2 The method is the same as in Example 1, except that the mixed micro-nano toughening particles in Example 1 are replaced with micron-sized aramid pulp (0.3 gsm). The I-mode interlaminar fracture toughness of the prepared fiber composite material is 1577.4 J / m 2 , compared with the reference sample of comparative example 1 (1577.9 J / m 2 ) is consistent, but significantly lower than Example 1 (1905.9 J / m 2 ); Mode II interlaminar fracture toughness is 1620.6 J / m 2 , compared with 1431.3 J / m 2 , which was increased by nearly 13.2%, but was significantly lower than Example 1 (1705.3 J / m 2 ).

[0051] Comparative Example 3 The method is the same as in Example 1, except that the mixed micro-nano toughening particles in Example 1 are replaced with nano-sized carbon nanotube particles (0.3 gsm). The I-mode interlaminar fracture toughness of the prepared fiber composite material is 1382.7 J / m 2 , which is significantly lower than the reference sample of Comparative Example 1 (1577.9 J / m 2 ) and Example 1 (1905.9 J / m 2 ); Mode II interlaminar fracture toughness is 1598.6 J / m 2 , compared with 1431.3 J / m 2 , which was increased by nearly 11.7%, but was significantly lower than Example 1 (1705.3 J / m 2 ).

[0052] Comparison test The fiber composite materials provided in the above Example 1 and Comparative Example 1 were tested as follows: 1) According to ASTM D5528, the evaluation of mode I interlaminar fracture toughness was carried out. The results are as follows Figure 5 and Figure 6 As shown, Figure 5 The double cantilever beam test results of the samples of Example 1 and Comparative Example 1 are shown in FIG. Figure 6 The R curves (crack extension resistance versus crack extension curves) of the samples of Example 1 and Comparative Example 1 show that compared with the reference sample of Comparative Example 1, the I-mode interlaminar fracture toughness of the composite material plate of Example 1 increases from 1577.9 J / m 2 Increased to 1905.9 J / m 2 , an increase of 20.79%.

[0053] 2) The Mode II interlaminar fracture toughness was evaluated according to ASTM D7905. Figure 7The end delamination flexure (ENF) test results of the samples of Example 1 and Comparative Example 1. The calculated Type II interlaminar fracture toughness of Example 1 is 1705.3 J / m 2 , compared with 1431.3 J / m 2 , an increase of nearly 19.1%.

[0054] Example 2 S1. Uniformly disperse the multi-scale structured mixed toughening particles in acetone solution Weigh 0.0188 g of micron-scale toughening particles aramid powder (Aramid-pulp) and nano-scale toughening particles carbon nanotubes (CNT), respectively, add them to a certain amount of acetone, and stir them evenly with a glass rod. Use an ultrasonic cell disruptor at room temperature (25°C) for 10 min to make the mixed micro-nano toughening particles disperse relatively evenly, and obtain a preliminarily dispersed mixed toughening particle acetone solution.

[0055] S2, spraying the acetone solution containing mixed micro-nano toughening particles on the unidirectional bismaleimide / carbon fiber prepreg Take the unidirectional bismaleimide / carbon fiber prepreg and cut a piece of 25 × 50 cm 2 The bismaleimide / carbon fiber prepreg is prepared by pouring the mixed micro-nano toughening particle acetone solution obtained in step S1 into a high atomization spray gun. The spray gun is connected to an air compressor (it is recommended to be equipped with an air purifier) ​​or a nitrogen bottle, the spraying pressure is 0.40 MPa, the spraying distance is 30 cm, and the mixed micro-nano toughening particle acetone solution is evenly sprayed on the bismaleimide / carbon fiber prepreg. Then, a breathable cloth is covered, the acetone is evaporated and dried, and a bismaleimide / carbon fiber prepreg containing 0.3 gsm mixed micro-nano toughening particles is prepared.

[0056] S3. Preparation of composite laminates Take the unidirectional bismaleimide / carbon fiber prepreg and cut it into 25×25 cm 2 size, and then manually stacked according to [0°] 20 The 10th and 11th layers of fiber cloth were laid in sequence, with one side of the fiber cloth covered with a mixed micro-nano toughening particle coating and arranged opposite to each other, and a 45 mm long PI film (30 μm thick) was laid in as a pre-crack.

[0057] The prepreg after laying is placed on a heating table and evaporated at 60 °C for 2 h to remove the remaining acetone solvent in the prepreg. After the solvent is completely evaporated, the preformed plate is moved as a whole into a flat vulcanizer for hot pressing. The curing conditions are: 100 °C / 30 min + 135 °C / 1 h + 150 °C / 30 min / 0.5 MPa + 180 °C / 1 h / 0.5 MPa + 235 °C / 2 h / 0.5 MPa + 255 °C / 6 h / 0.5 MPa. After that, it is cooled and demolded to obtain a composite laminate.

[0058] The plates were cut into appropriate sizes according to the test standards, and then subjected to hinged double cantilever beam (DCB) test and end delamination flexure (ENF) test respectively, to measure the mode I interlaminar fracture toughness (G IC ) is 402.9 J / m 2 , compared to the baseline sample without any toughening particles (337.9 J / m 2 ) was increased by about 19.2%; Type II interlaminar fracture toughness (G IIC ) is 1402.3 J / m 2 , compared to the baseline sample without any toughening particles (903.2 J / m 2 ) increased by about 55.26%.

[0059] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0060] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A method for preparing an interlayer toughened fiber composite material, characterized in that: include: Dispersing micron-sized toughening particles and nano-sized toughening particles in a solvent to form a mixed toughening particle dispersion; wherein the solvent is a low-viscosity, volatile solvent; Also, the mixed toughening particle dispersion is applied to the fiber cloth by spraying, and then compounded with resin and cured to obtain an interlayer toughening fiber composite material; or, the mixed toughening particle dispersion is applied to the prepreg by spraying, and then cured to obtain an interlayer toughening fiber composite material.

2. The preparation method according to claim 1, characterized in that: The micron-sized toughening particles include micron-sized aramid pulp; preferably, the micron-sized aramid pulp includes interfacially modified aramid pulp and / or non-interfacially modified aramid pulp; And / or, the particle size of the micron-sized toughening particles is 50-200 μm; And / or, the nano-scale toughening particles include carbon nanotubes; preferably, the carbon nanotubes include surface-modified carbon nanotubes and / or non-surface-modified carbon nanotubes; preferably, the carbon nanotubes include carbon nanotubes with functional groups grafted on the surface, wherein the functional groups include any one or more combinations of carboxyl, amino, and hydroxyl groups; And / or, the particle size of the nanoscale toughening particles is 10-50 nm.

3. The preparation method according to claim 1, characterized in that: The solvent includes any one or more combinations of water, alcohol, and acetone; And / or, the usage ratio of the micron-sized toughening particles, nano-sized toughening particles and the solvent is 0.01-0.03 g: 0.01-0.03 g: 100 ml.

4. The preparation method according to claim 1, characterized in that: Specifically include: Using a high-pressure spray gun device to evenly spray the mixed toughening particle dispersion on the fiber cloth, and wait for the solvent to evaporate to obtain a modified fiber cloth; stacking and arranging a plurality of modified fiber cloths to form a fiber preform; Furthermore, the resin and the curing agent are mixed to form a resin-based slurry, and the resin-based slurry is then introduced into a fiber preform, and then cured and formed to obtain an interlayer toughened fiber composite material.

5. The preparation method according to claim 4, characterized in that: The fiber cloth includes any one or more combinations of carbon fiber cloth, glass fiber cloth, basalt cloth, and aramid fiber cloth; And / or, the fiber cloth includes any one of unidirectional fiber cloth, bidirectional fiber cloth, and three-dimensional fiber cloth; And / or, the resin includes any one or more combinations of epoxy resin, polyester, phenolic resin, vinyl ester, bismaleimide, and thermoplastic resin.

6. The preparation method according to claim 1, characterized in that: Specifically include: Using a high-pressure spray gun device to evenly spray the mixed toughening particle dispersion on the prepreg, and after the solvent evaporates, a modified prepreg is obtained; Furthermore, a plurality of modified prepregs are stacked and arranged, and then cured and formed to obtain an interlayer toughened fiber composite material.

7. The preparation method according to claim 6, characterized in that: The prepreg includes bismaleimide resin / carbon fiber prepreg and / or epoxy resin / carbon fiber prepreg.

8. The preparation method according to claim 1, characterized in that: The curing molding includes any one of VARTM, RTM, hand lay-up molding, compression molding, and autoclave molding.

9. An interlaminar toughened fiber composite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the interlaminar toughened fiber composite material according to claim 9 in the fields of automobiles, aerospace or ships.

Citation Information

Cited By

  • Prepreg and preparation method thereof

    CN121495350A

  • Fiber-reinforced resin-based composite material with damping and impact resistance as well as preparation method and application of fiber-reinforced resin-based composite material

    CN122518747A