A method for preparing graphene powder

By improving the Hummers method to prepare graphene oxide and then subjecting it to chemical reduction and high-temperature calcination, the problem of preparing low-layer-number graphene powder in existing technologies has been solved, enabling the large-scale preparation and high conductivity application of graphene powder, thus meeting the requirements of high energy density and fast charging performance of lithium batteries.

CN118908194BActive Publication Date: 2026-11-17THE SIXTH ELEMENT CHANGZHOU MATERIALS TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411144618.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2026-11-17
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Existing technologies are insufficient for efficiently preparing low-layer-number graphene materials, and dispersants have adverse effects in lithium-ion batteries, failing to meet the requirements for high energy density and fast charging performance.

Method used

Graphene oxide (GO) was prepared by modifying the Hummers method, controlling its concentration and number of layers in water, and then reducing graphene oxide (rGO) was obtained by chemical reduction. Finally, oligolayer graphene powder was prepared by stirring and high-temperature calcination.

Benefits of technology

The large-scale preparation of graphene powder has been achieved, which improves conductivity, meets the requirements of high energy density and fast charging performance of lithium batteries, and solves the problem of the adverse effects of dispersants in batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908194B_ABST
    Figure CN118908194B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing graphene powder, comprising the following steps: preparing graphene oxide, wherein the number of layers of the graphene oxide is ≤3; preparing a graphene oxide dispersion using the graphene oxide; reducing, separating, and drying the graphene oxide dispersion to obtain a reduced graphene oxide solid; performing a fluffing treatment on the reduced graphene oxide solid to obtain fluffy reduced graphene oxide powder; and calcining the fluffy reduced graphene oxide powder at high temperature to obtain graphene powder. The graphene prepared by this invention bridges some of the gap between the conductivity of commercially available graphene powder and theoretical graphene, further enhancing the practical application value of graphene, providing favorable support for achieving high energy density and faster charging performance in lithium batteries, realizing the large-scale preparation of graphene powder, and meeting the requirements of downstream applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thin-layer graphene material preparation, and more particularly to a method for preparing low-layer-number graphene. Background Technology

[0002] Graphene is a material composed of carbon atoms through sp... 2 The two-dimensional, honeycomb-like layered structure formed by hybridization is the basic structural unit of other carbon materials. Since its discovery, it has been a research hotspot in the field of materials science due to its outstanding physicochemical properties.

[0003] Oligolayer graphene generally refers to graphene with fewer than 5 layers. Compared to other multilayer graphene, oligolayer graphene is thinner and more flexible, exhibiting outstanding performance in nanoelectronic devices and composite materials. Adding oligolayer graphene to batteries can increase conductivity, thereby enhancing battery capacity and cycle life.

[0004] There are various methods for preparing graphene, including mechanical exfoliation, liquid phase exfoliation, chemical oxidation, crystal epitaxial growth, chemical vapor deposition, organic synthesis, and carbon nanotube exfoliation.

[0005] Mechanical exfoliation overcomes the inter-sheet forces in graphite by mechanical means and uses photoresist to separate the graphite, successfully obtaining single-layer graphene. Although this method can produce graphene with fewer layers than conventional mechanical exfoliation, it still struggles to precisely control the purity of graphene and has extremely low yields, making large-scale graphene production difficult. Currently, commercially available mechanical exfoliation methods for preparing graphene slurries typically use mills, homogenizers, and other equipment to break down and exfoliate the graphite. The resulting graphene material is generally ≥10 layers thick, classifying it as multilayer graphene. This method cannot produce few-layer or oligolayer graphene. Furthermore, these methods require the addition of small amounts of dispersants to stabilize the graphene during the breaking down and exfoliation process. These dispersants can have adverse effects in downstream lithium-ion battery applications, hindering the development of more advanced graphene materials.

[0006] Liquid-phase exfoliation involves using ultrasonic waves, heating, or other methods to exfoliate graphite, preparing single-layer or multi-layer graphene solutions. This method requires the addition of numerous dispersants during graphene preparation. These dispersants stabilize the graphene sheets in the solution. However, in downstream lithium-ion battery manufacturing, the dispersants on the graphene surface, acting as conductive agents, cannot be separated, resulting in dispersants remaining in the electrodes during positive and negative electrode assembly. The presence of these dispersants reduces the high-voltage withstand capability of the assembled battery. The fundamental reason is that dispersants are often high-molecular-weight or low-molecular-weight materials that decompose under high voltage and high current, producing gases and undergoing cyclic expansion and other adverse phenomena. Therefore, they are unsuitable for high-current charging and discharging. In today's fast-paced lifestyle, the conductive agents in this method are insufficient to meet the demands of fast charging.

[0007] Chemical vapor deposition (CVD) involves decomposing carbon-containing chemicals (such as methane) at high temperatures. The resulting carbon atoms are deposited on a substrate, where they combine to form graphene. This method can produce single-layer or even monolayer graphene materials. Transparent graphene films can be used in electronic touchscreens, sensors, transistors, and more. The main hurdle is how to peel the graphene from the substrate without damage or contamination, which remains a key challenge. Furthermore, CVD is not suitable for preparing graphene powder materials, and the resulting graphene cannot be used as a conductive agent in lithium-ion batteries.

[0008] Epitaxial growth, organic synthesis, and carbon nanotube exfoliation are all methods that can produce single-layer and few-layer graphene materials, but cost and large-scale production remain limiting factors.

[0009] The oxidation-reduction method involves chemically oxidizing and exfoliating graphene to obtain graphene oxide (GO) with a high monolayer ratio, and then reducing GO to obtain graphene. This method is the optimal route for preparing graphene powder with a high monolayer ratio. Summary of the Invention

[0010] To address the above problems, this invention provides a method for preparing oligolayer graphene, comprising the following steps:

[0011] S1: Prepare graphene oxide, wherein the graphene oxide satisfies the following conditions:

[0012] The graphene oxide dispersion with a concentration of 50 ppm has an absorption peak at 230 nm ≥ 2.0;

[0013] S2: Prepare a graphene oxide dispersion using the graphene oxide from step S1;

[0014] S3: Reduce, separate, and dry the graphene oxide dispersion from step S2 to obtain a solid.

[0015] S4: The solid obtained in step S3 is subjected to a fluffing treatment to obtain fluffy powder;

[0016] S5: The fluffy powder described in step S4 is calcined at high temperature to obtain graphene powder.

[0017] Preferably, in step S1, the number of graphene oxide layers is ≤3.

[0018] Preferably, the graphene oxide dispersion with a concentration of 50 ppm has an absorption peak of 2.0-3.5 at 230 nm, such as 2.1, 2.5, 2.6, 2.8, 3.2, 3.5, etc.

[0019] Preferably, in step S2, the solid content of the graphene oxide dispersion is ≤0.1wt%, more preferably 0.02-0.1wt%, such as 0.02, 0.05, 0.09, 0.1, 0.25, 0.3, 0.35, etc.

[0020] Preferably, the viscosity of the graphene oxide dispersion is ≤1500 mPa·s; more preferably, it is 50-800 mPa·s.

[0021] Preferably, in step S3, the method for reducing the graphene oxide dispersion in step S2 is: to perform reduction using a redox method.

[0022] Preferably, the reducing agent in the redox method is one or more of an organic compound containing -NH2, a phenol or alcohol containing -OH, a metal hydride, or a hydrogen halide, such as a monohydric alcohol, a polyhydric alcohol, a monohydric phenol, a polyhydric phenol, NaBH4, LiAlH4, hydroiodic acid, hydrobromic acid, etc.

[0023] Preferably, the mass ratio of graphene oxide to reducing agent is 1:(2-6), for example 1:2, 1:3, 1:2.5, 1:3.5, 1:4, 1:5, 1:5.5, 1:6, etc.; more preferably 1:(3-5).

[0024] Preferably, the reduction temperature is 50-100℃ and the stirring reaction time is 2-12h; more preferably, the temperature is 50-80℃ and the stirring reaction time is 8-12h.

[0025] Preferably, the water content of the solid obtained by drying is ≤5 wt%.

[0026] Preferably, the separation method is filtration separation or centrifugal separation.

[0027] Preferably, step S3 further includes reducing and separating the graphene oxide dispersion from step S2, followed by purification.

[0028] Preferably, the purification is performed 1-4 times.

[0029] Preferably, in step S4, the method for fluffing is to stir the solid obtained in step S3 in a stirrer.

[0030] Preferably, the stirring speed is 500-2000 rpm and the stirring time is 0.15-3 h; more preferably, the stirring speed is 1000-2000 rpm and the stirring time is 0.5-2 h.

[0031] Preferably, the tap density of the loose powder is 0.01-0.1 g / cm³. 3 Further preferably, it is 0.05-0.09 g / cm³. 3 .

[0032] Preferably, in step S5, the high-temperature calcination temperature is 1000-1500℃ and the calcination time is 1-4h; more preferably, the temperature is 1000-1300℃ and the calcination time is 2-4h.

[0033] This invention also protects a graphene powder prepared by a specific method.

[0034] Preferably, the graphene powder has ≤5 layers.

[0035] The working principle of this invention is as follows: GO raw materials are prepared in batches using a modified Hummers method. Then, by reducing the concentration of GO in water, a thin layer of GO is obtained, thus reducing agglomeration after reduction. After reduction with chemical reagents, the obtained rGO is separated; at this point, the rGO can be stably dispersed in water. After drying, rGO powder is obtained. However, simple drying would result in rGO agglomerates. Therefore, the rGO powder is subjected to high-speed stirring in a sealed container to fluff it up, achieving a dispersion effect and preventing the dried rGO powder from agglomerating, resulting in a thin layer of rGO powder. Finally, this thin layer of rGO is directly subjected to high-temperature repair to obtain oligolayer graphene powder material. In the above process, by controlling the preparation of the thin layer of rGO and fluffing the rGO powder, the rGO powder before high-temperature repair achieves a thin layer effect. Subsequent high-temperature repair yields oligolayer graphene powder, realizing the large-scale preparation of graphene powder and meeting the requirements of downstream applications.

[0036] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0037] (1) The development of graphene powder materials has made up for some of the gap between the conductivity of graphene powder on the market and that of theoretical graphene, and further enhanced the practical application value of graphene.

[0038] (2) It provides favorable support for lithium batteries to achieve high energy density and higher fast charging performance;

[0039] (3) Achieve large-scale preparation of graphene powder to meet the requirements of downstream applications. Attached Figure Description

[0040] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings:

[0041] Figure 1 This is a schematic diagram of the graphene preparation method provided by the present invention;

[0042] Figure 2 This is an atomic force microscope image of the raw material GO in an embodiment of the present invention;

[0043] Figure 3 This is a scanning electron microscope image of graphene obtained by the preparation method of the embodiments of the present invention;

[0044] Figure 4 This is a transmission electron microscope image of graphene obtained by the preparation method of the present invention. Detailed Implementation

[0045] To facilitate understanding of the present invention, a more complete description will be provided below. Preferred embodiments of the invention are given below. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the invention.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0047] This document refers to numerical ranges, which, unless otherwise specified, are considered continuous and include the minimum and maximum values ​​of the range, as well as every value between them. Furthermore, when a range refers to an integer, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0048] Unless otherwise specified, the temperature parameters in this document can be either constant temperature processing or processing within a certain temperature range. The constant temperature processing allows for temperature fluctuations within the precision range controlled by the instrument.

[0049] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0050] like Figure 1 This is a schematic diagram of the method for preparing oligolayer graphene provided by the present invention.

[0051] This invention provides a method for preparing oligolayer graphene, comprising the following steps:

[0052] (1) Selection of raw material GO

[0053] In order to achieve good dispersion of GO at a solid content of ≤0.1%, GO itself needs to be easily dispersed, so the GO itself needs to have a relatively high monolayer ratio. At the same time, GO has a high affinity for water, so the raw material GO needs to have a high degree of oxidation and a high degree of exfoliation.

[0054] To select the GO raw material with the required low number of layers, the method used is to test the solubility of GO in water. Specifically, GO is dispersed in water to obtain a dispersion with a concentration of 50 ppm. The absorption peak value of the dispersion at 230 nm is measured using a UV-Vis (ultraviolet-visible absorption spectrometer). When the absorption peak value is ≥2.0, it meets the requirement of good water dispersion of GO to a low number of layers; preferably, the absorption peak value range is 2.0-3.5. In this invention, the number of GO layers after dispersion is ≤3.

[0055] To further confirm whether the selected raw material GO is of a low layer number, it can be tested using an atomic force microscope, such as... Figure 2 As shown in the figure, the raw material GO is basically in a single-layer state.

[0056] In this invention, the number of layers of raw material GO refers to the number of layers when raw material GO is dispersed in a dispersion with a concentration of 50 ppm.

[0057] (2) Preparation of low-concentration GO dispersion

[0058] The GO is prepared into an aqueous dispersion with a solid content ≤0.1wt%, preferably 0.02-0.1wt%. The GO dispersion is prepared into a dispersion with a viscosity ≤1500mPa·s, preferably 50-800mPa·s, by means of stirring dispersion, homogenization dispersion, microfluidization, etc., to ensure that GO can be uniformly dispersed in the aqueous solution.

[0059] The solid content mentioned above refers to the percentage by mass of the emulsion or coating remaining after drying under specified conditions.

[0060] When the solid content is >0.1%, the aqueous dispersion of GO is not easily dispersed into a monolayer or few-layer state. During reduction, the layers are prone to agglomeration, which can easily lead to the prepared rGO having more than 5 layers, thus failing to obtain oligolayer graphene. When the solid content is ≤0.1%, the viscosity is ≤1500 mPa·s. The viscosity is too high, which will cause uneven reaction of the reducing agent added later.

[0061] (3) Reduction of GO dispersion

[0062] A chemical reducing agent is added to the above GO dispersion, with a GO solid to chemical reducing agent mass ratio of 1:(2-6); preferably, 1:(3-5). The mixture is stirred at 50-100℃ for 2-12 hours to obtain a black flocculent liquid, from which a black solid is separated; preferably, the temperature is 50-80℃ and the stirring time is 8-12 hours. The black solid is then purified by washing it with water 1-4 times.

[0063] When the mass ratio of solid GO to chemical reducing agent is less than 1:2, GO is not reduced completely, leading to incomplete repair during subsequent high-temperature treatment. Furthermore, the resulting rGO exhibits a more pronounced aggregation effect because the hydrogen bonds between GO atoms accelerate aggregation. When the ratio is greater than 1:6, besides wasting resources, excess reducing agent remains on the rGO. Adding excessive reducing agent to the GO solution causes GO aggregation, making it impossible to prepare oligolayer graphene materials.

[0064] When the temperature is below 50℃, the reduction effect will be reduced; if the temperature is too high, GO or rGO (redox graphene) in the resulting solution will agglomerate.

[0065] When the stirring time is 2-12 hours, the reaction can proceed fully within this timeframe. Stirring for longer than this time will result in energy waste and reduced efficiency.

[0066] Among them, the chemical reducing agents include -NH2 organic compounds, phenols and alcohols containing -OH (monohydrins, polyhydrins, monohydric phenols, polyphenols), metal hydrides (NaBH4, LiAlH4, etc.), hydrogen halides (hydroiodic acid, hydrobromic acid), etc., and can be one or more of the above chemical reducing agents, which can be selected according to actual needs.

[0067] There are many methods to separate black flocculent liquid into black solids, such as filtration and centrifugation. Any method that can achieve the separation purpose is acceptable and will not be limited here.

[0068] (4) The purified black solid was dried and fluffed.

[0069] The purified black solid was dried in an oven to obtain rGO powder. The water content of the dried solid was ≤5wt%.

[0070] When the moisture content of the solid is within the above range, the solid will be in a blocky state, and it will be fully fluffed during subsequent high-speed stirring. When the moisture content is higher than 5 wt%, the solid may stick to the stirring device and cannot be fully fluffed, thus failing to achieve the purpose of fluffing.

[0071] The mixture is stirred in a high-speed mixer, such as the stirring device described in patent CN213611236U, at a speed of 500–2000 rpm for 0.15–3 hours. Preferably, the stirring speed is 1000–2000 rpm for 0.5–2 hours. Within this range, the solid can be sufficiently fluffed, allowing the rGO to disperse as much as possible, preparing for subsequent high-temperature graphitization to obtain graphene powder with ≤5 layers. Utilizing the principle of stirring and convection, the dried rGO black agglomerates are subjected to a fluffing treatment. Before fluffing, the tap density of the rGO black agglomerates is 0.1–0.4 g / cm³. 3 After fluffing treatment, the resulting fluffy rGO powder had a tap density of 0.01-0.1 g / cm³. 3 Preferably, it is 0.05–0.09 g / cm³. 3 .

[0072] Tapped density refers to the mass per unit volume of powder in a container after it has been tapped under specified conditions.

[0073] (5) High-temperature repair of fluffy rGO powder to obtain graphene powder.

[0074] Loose rGO powder is calcined in a high-temperature furnace under inert conditions, with the temperature increased to 1000–1500°C at a rate of 5°C / min, and heat-treated for 1–4 hours to obtain oligolayer graphene powder material; preferably, the temperature is 1000–1300°C and the calcination time is 2–4 hours. Figure 3 , Figure 4 As shown.

[0075] When the temperature is below 1000℃, it is insufficient to completely eliminate the oxygen-containing functional groups on rGO, so the defects caused by O atoms cannot be completely repaired; when the temperature is above 1500℃, a rearrangement reaction of C atoms will occur, which will repair the graphene two-dimensional sheet structure with a complete lattice. At this time, the graphene sheets overlap (due to π-π forces).

[0076] The graphene powder prepared by the above method was tested using the following methods:

[0077] The test method for the mass fraction of C and O elements is: DB32 / T 3595-2019.

[0078] The testing method for ID / IG is: Q / NGSIC 012-2020.

[0079] The test method for specific surface area (BET) is GB / T 7702.20-1997.

[0080] The test method for oil absorption value is GBT 3780.2-2007.

[0081] The conductivity testing method is described in Sasha Stankovich, Dmitriy A. Dikin, et al., Synthesis of graphene-based nanosheets via chemical reduction of exfoliated graphite oxide, Carbon 45 (2007): [lines 1558-1565]. The conductivity of graphene powder was tested using the method described in this literature.

[0082] The test results are shown in Table 1.

[0083] Table 1 Performance data of graphene powder prepared by the method of the present invention

[0084]

[0085] As shown in Table 1, C (wt%) ≥ 97.2% and O (wt%) ≤ 0.05%, indicating that the GO raw material was almost completely reduced to form graphene; ID / IG ≤ 1.05 indicates that the defect degree of the graphene after thermal repair is low; BET ≥ 750m 2 The / g indicates that the graphene prepared by this method has a relatively large specific surface area. Furthermore, based on the theoretical specific surface area calculation for graphene, a specific surface area of ​​750m² is considered optimal. 2 At a density of / g, the average number of graphene layers is around 3. This indicates that the BET of graphene powder is ≥750m. 2 The graphene content is / g, indicating it is oligolayer graphene; the oil absorption value is between 3500 and 5500 ml / 100g, indicating that the graphene powder material has a large specific surface area, and the larger the oil absorption value, the larger the specific surface area, and vice versa; the electrical conductivity range is 10. 5 ~10 6 The S / m ratio indicates that the prepared graphene powder has good electrical conductivity.

[0086] The present invention will be further described below with reference to specific embodiments.

[0087] Example 1:

[0088] A method for preparing graphene powder:

[0089] Prepare GO raw materials with ≤3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 2.08 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.05%. After stirring evenly, add 15 g of vitamin C, heat to 80℃, and continue stirring for 5 h. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500 rpm for 30 min to obtain a fluffy black rGO powder. Place the black rGO powder in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1000℃ at a heating rate of 5℃ / min, and heat-treat for 4 h to obtain graphene powder. The performance of the graphene powder was tested, as shown in Table 2.

[0090] Example 2:

[0091] A method for preparing graphene powder:

[0092] Prepare GO raw materials with ≤3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 2.06 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.02%. After stirring evenly, add 10 g of ethylenediamine, heat to 50℃, and continue stirring for 3 h. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1000 rpm for 30 min to obtain a fluffy black rGO powder. Place the black rGO powder in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1100℃ at a heating rate of 5℃ / min, and heat-treat for 3 h to obtain graphene powder. The performance of the graphene powder was tested, as shown in Table 2.

[0093] Example 3:

[0094] A method for preparing graphene powder:

[0095] Prepare GO raw materials with ≤3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 2.07 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.1%. After stirring evenly, add 10 g of vitamin C, heat to 65℃, and continue stirring for 8 hours. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500 rpm for 30 minutes to obtain a fluffy black rGO powder. Place the black rGO powder in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1400℃ at a heating rate of 5℃ / min, and heat-treat for 2 hours to obtain graphene powder. The performance of the graphene powder was tested, as shown in Table 2.

[0096] Example 4:

[0097] A method for preparing graphene powder:

[0098] Prepare GO raw materials with ≤3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 2.12 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.01%. After stirring evenly, add 23 g of vitamin C, heat to 95℃, and continue stirring for 2 h. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500 rpm for 30 min to obtain a fluffy black rGO powder. Place the black rGO powder in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1500℃ at a heating rate of 5℃ / min, and heat-treat for 1 h to obtain graphene powder. The performance of the graphene powder is tested, as shown in Table 2.

[0099] Example 5:

[0100] A method for preparing graphene powder:

[0101] Prepare GO raw materials with ≤3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 2.14 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.01%. After stirring evenly, add 10 g of hydroiodic acid, heat to 50℃, and continue stirring for 2 h. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1000 rpm for 30 min to obtain a fluffy black rGO powder. Place the black rGO powder in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1300℃ at a heating rate of 5℃ / min, and heat-treat for 2.5 h to obtain graphene powder. The performance of the graphene powder was tested, as shown in Table 2.

[0102] Comparative Example 1:

[0103] A method for preparing graphene powder:

[0104] Prepare GO raw materials with more than 3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 1.03 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.05%. After stirring evenly, add 15 g of vitamin C (Vc), heat to 80℃, and continue stirring for 5 h. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500 rpm for 30 min to obtain a fluffy black rGO powder. Place the black rGO powder in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1300℃ at a heating rate of 5℃ / min, and heat-treat for 2.5 h to obtain graphene powder. The performance of the graphene powder was tested, as shown in Table 2.

[0105] Comparative Example 2:

[0106] A method for preparing graphene powder:

[0107] Prepare GO raw materials with ≤3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 2.08 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.05%. After stirring evenly, add 15 g of vitamin C (Vc), heat to 80℃, and continue stirring for 5 h. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the black rGO solid in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1300℃ at a heating rate of 5℃ / min, and heat-treat for 2.5 h to obtain graphene powder. The performance of the graphene powder is tested, as shown in Table 2.

[0108] Comparative Example 3:

[0109] A method for preparing graphene powder:

[0110] Prepare GO raw materials with more than 3 layers (a dispersion of GO in water with a concentration of 50 ppm and an absorption peak of 1.03 at 230 nm). Take 5 g of the dispersion to prepare an aqueous dispersion with a GO solid content of 0.05%. After stirring evenly, add 15 g of vitamin C, heat to 80℃, and continue stirring for 5 h. Then separate the resulting reaction solution to obtain reduced rGO. Wash twice with water and dry in an oven to obtain a solid. Place the black rGO solid in a high-temperature calcination furnace under nitrogen atmosphere, raise the temperature to 1300℃ at a heating rate of 5℃ / min, and heat-treat for 2.5 h to obtain graphene powder. The performance of the graphene powder was tested, as shown in Table 2.

[0111] Table 2. Performance data of graphene prepared in the examples and comparative examples.

[0112]

[0113]

[0114] Comparing Example 1 with Comparative Example 1, it is shown that when the number of GO layers in the raw material is greater than 3, the resulting graphene powder has a significantly lower specific surface area than graphene with a low number of GO layers (≤3 layers), and cannot be made into a few-layer graphene material.

[0115] Compared with Comparative Example 2, in Example 1, graphene powder with a high specific surface area could not be obtained without fluffing the rGO obtained in the intermediate process.

[0116] Compared with Comparative Example 3, Example 1 shows that when the number of GO layers in the raw material is not controlled and the rGO obtained in the intermediate process is not fluffed, the resulting graphene powder material has a lower specific surface area, and it is impossible to obtain graphene powder with a high specific surface area.

[0117] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0118] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for preparing graphene powder, characterized in that, Includes the following steps: S1: Prepare graphene oxide, wherein the graphene oxide satisfies the following conditions: The absorption peak value of the graphene oxide dispersion with a concentration of 50 ppm at 230 nm is ≥2.

0. S2: Prepare a graphene oxide dispersion using the graphene oxide from step S1, wherein the solid content of the graphene oxide dispersion is ≤0.1wt%; S3: Reduce, separate, and dry the graphene oxide dispersion in step S2 to obtain a solid, the water content of which is ≤5wt%; the method for reducing the graphene oxide dispersion in step S2 is to use an oxidation-reduction method. S4: The solid obtained in step S3 is subjected to a fluffing treatment to obtain a fluffy powder; the fluffing treatment method is as follows: the solid obtained in step S3 is stirred in a stirrer; the stirring speed is 500~2000 rpm, and the stirring time is 0.15~3 h; the tap density of the fluffy powder is 0.01-0.1 g / cm³. 3 ; S5: The fluffy powder obtained in step S4 is subjected to high-temperature calcination to obtain graphene powder. The high-temperature calcination temperature is 1000-1500℃ and the calcination time is 1-4h.

2. The preparation method according to claim 1, characterized in that, In step S1, the number of graphene oxide layers is ≤3; the absorption peak value of the graphene oxide dispersion with a concentration of 50ppm at 230nm is 2.0-3.

5.

3. The preparation method according to claim 1, characterized in that, In step S2, the solid content of the graphene oxide dispersion is 0.02-0.1 wt%.

4. The preparation method according to claim 1, characterized in that, The viscosity of the graphene oxide dispersion is ≤1500 mPa·s.

5. The preparation method according to claim 4, characterized in that, The viscosity of the graphene oxide dispersion is 50-800 mPa·s.

6. The preparation method according to claim 1, characterized in that, In step S3, the reducing agent used in the redox method is one or more of the following: an organic compound containing -NH2, a phenol or alcohol containing -OH, a metal hydride, or a hydrogen halide.

7. The preparation method according to claim 1, characterized in that, In step S3, the mass ratio of graphene oxide to reducing agent is 1:(2-6).

8. The preparation method according to claim 7, characterized in that, The mass ratio of graphene oxide to reducing agent is 1:(3-5).

9. The preparation method according to claim 1, characterized in that, In step S3, the reduction temperature is 50-100℃, and the stirring reaction time is 2-12h.

10. The preparation method according to claim 9, characterized in that, The reduction temperature is 50-80℃, and the stirring reaction time is 8-12h.

11. The preparation method according to claim 1, characterized in that, The separation method is either filtration or centrifugation.

12. The preparation method according to claim 1, characterized in that, Step S3 also includes reducing and separating the graphene oxide dispersion from step S2, followed by purification; the purification is performed 1-4 times.

13. The preparation method according to claim 1, characterized in that, In step S4, the stirring speed is 1000-2000 rpm, and the stirring time is 0.5-2 hours; the tap density of the loose powder is 0.05-0.09 g / cm³. 3 .

14. The preparation method according to claim 1, characterized in that, In step S5, the high-temperature calcination temperature is 1000-1300℃, and the calcination time is 2-4h.

Citation Information

Patent Citations

  • Mixing granulation equipment

    CN213611236U

  • Preparing method of oxidized graphene and high-conductivity graphene

    CN106564891A

  • Quantitative characterization method for dispersion degree of graphene oxide and characterization model for dispersion degree of graphene oxide

    CN108693129A