Bamboo-based activated carbon manufacturing method and manufacturing device

By optimizing the slice and oxygen-free charring process of bamboo, using the condensation tower to collect pyrolytic gas for recycling, the problem of high ash content and poor strength of bamboo activated carbon is solved, and the preparation of bamboo charcoal with high strength and low ash is achieved, which satisfies the further High application standards.

CN118908203APending Publication Date: 2024-11-08XIAMEN QIANQI NEW MATERIALS TECHNOLOGY RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410971889.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing bamboo activated carbon has a high ash content and poor strength, which limits its use in practical applications.

Method used

By slicing bamboo, bamboo green and bamboo yellow were obtained, and pyrolyzed in an oxygen-free charcoal furnace. The pyrolyzed gas was collected and circulated by the condensation tower, and the pyrolyzed temperature and time were controlled to obtain high-intensity, low-ash bamboo carbonization material.

Benefits of technology

It significantly improves the strength of bamboo charcoal, reduces the ash content, meets higher application standards, increases the strength to 93-99%, and reduces the ash content to <3%, solving the problems of poor strength and high ash content of existing bamboo activated carbon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908203A_ABST
    Figure CN118908203A_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing method and a manufacturing device of bamboo activated carbon. The manufacturing method comprises the following steps: slicing bamboos to obtain bamboo green and tabasheer of the bamboos; placing the bamboo green or tabasheer part of the bamboo in a furnace pipe of an oxygen-free furnace, introducing natural gas into a hearth in a furnace body outside the furnace pipe of the oxygen-free furnace, pyrolyzing the bamboo green or tabasheer part to 260-280 DEG C, and introducing pyrolysis gas in the furnace pipe into a cooling tower; the cooling tower exhausts the pyrolysis gas with the temperature lower than 260 DEG C to the outside, the gas with the temperature higher than 260 DEG C is introduced into the hearth again to form pyrolysis gas circulation, and fire is turned off; and the bamboo green part or the tabasheer part is controlled to be pyrolyzed for 40-90 minutes or 40-60 minutes in the furnace pipe. According to the technical scheme, fragmentation and utilization of bamboos are achieved, recycling of heat energy contained in combustible gas generated after pyrolysis of the bamboos is achieved, and the recycling is combined with pyrolysis of bamboo charcoal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of activated carbon production, and in particular to a method and a device for producing bamboo activated carbon. Background Art

[0002] The preparation of activated carbon generally uses coal, fruit shells, and charcoal as the main raw materials. Bamboo activated carbon is a new material. Bamboo is widely available and inexpensive, making it an excellent material for making activated carbon. However, due to the limitations of the process and the characteristics of bamboo itself, bamboo activated carbon has a high ash content and poor strength, which is subject to many restrictions in practical applications. Summary of the invention

[0003] In view of the above problems, the present invention provides a method and a device for producing bamboo activated carbon, which solve the problem of excessively high ash content in the existing bamboo activated carbon firing process.

[0004] To achieve the above object, in a first aspect, the present invention provides a method for preparing bamboo activated carbon, the method comprising:

[0005] The bamboo is sliced ​​to obtain bamboo green and bamboo yellow;

[0006] The green part of bamboo is placed in the furnace of an oxygen-free carbonization furnace, natural gas is ignited in the furnace inside the furnace body outside the furnace of the oxygen-free carbonization furnace, and the bottom of the furnace containing the green bamboo is heated until the temperature of the pyrolysis gas in the furnace reaches 260°C-280°C;

[0007] If the temperature of the pyrolysis gas is less than 260° C., the pyrolysis gas is directly discharged to the outside, and / or is discharged to the outside after being collected by the bamboo vinegar liquid in the condensation tower;

[0008] If the pyrolysis gas is discharged directly to the outside, the valve should be switched to discharge steam outside before entering the condensation tower;

[0009] If the temperature of the pyrolysis gas is greater than or equal to 260°C, the pyrolysis gas is introduced into the furnace through the condensation tower for spontaneous combustion to form a pyrolysis gas cycle, and the natural gas is cut off;

[0010] The green bamboo part is controlled to be pyrolyzed in the furnace for 40-90 minutes to obtain high-strength bamboo charcoal carbonized material.

[0011] In some embodiments, controlling the pyrolysis of the green bamboo part in the furnace for 40-90 minutes further comprises:

[0012] During the pyrolysis process of the green bamboo part, the temperature in the furnace is controlled within the range of 500-650°C.

[0013] In some embodiments, the method comprises:

[0014] The bamboo yellow part of the bamboo is placed in the furnace of the oxygen-free carbonization furnace, and natural gas is ignited in the furnace area inside the furnace body outside the furnace of the oxygen-free carbonization furnace to heat the bottom of the furnace containing the bamboo yellow until the temperature of the pyrolysis gas in the furnace reaches 260°C-280°C;

[0015] If the temperature of the pyrolysis gas is less than 260° C., the pyrolysis gas is directly discharged to the outside, and / or is discharged to the outside after being collected by the bamboo vinegar liquid in the condensation tower;

[0016] If the pyrolysis gas is discharged directly to the outside, the valve should be switched to discharge steam outside before entering the condensation tower;

[0017] If the temperature of the pyrolysis gas is greater than or equal to 260°C, the pyrolysis gas is introduced into the furnace through the condensation tower for spontaneous combustion to form a pyrolysis gas cycle, and the natural gas is cut off;

[0018] The green bamboo part is controlled to be pyrolyzed in the furnace for 40-90 minutes to obtain high-strength bamboo charcoal carbonized material.

[0019] The bamboo yellow part is controlled to be pyrolyzed in the furnace for 40-60 minutes to obtain low-ash bamboo charcoal carbonized material.

[0020] In some embodiments, controlling the pyrolysis of bamboo yellow in the furnace for 40-60 minutes further comprises:

[0021] The temperature of bamboo yellow pyrolysis in the furnace is in the range of 500-550℃.

[0022] In a second aspect, the present invention provides a bamboo activated carbon production device, which is applicable to the method described in the first aspect, and the production device comprises:

[0023] An oxygen-free carbonization furnace comprises a furnace body, a furnace core and a furnace chamber, wherein the space between the outside of the furnace core and the inside of the furnace body is a combustion space, namely, the furnace chamber, the furnace core is provided with a first air outlet above, the side wall of the furnace body is provided with a first air inlet, and the first air inlet is connected to the furnace chamber;

[0024] A burner, the burner is placed at the bottom of the furnace and is used to heat the furnace;

[0025] A condensation tower, comprising a first delivery port and a second delivery port, wherein the first delivery port is connected to the first air outlet, and the second delivery port is connected to the first air inlet;

[0026] A three-way pipe is arranged at the connection point between the first gas outlet and the first delivery port, and the other end of the three-way pipe is connected to the outside;

[0027] The valve group includes a first valve, a second valve and a third valve, wherein the first valve is arranged at the connection between the second delivery port and the first air inlet, the second valve is arranged at the connection between the three-way pipe and the first delivery port, and the third valve is placed on the pipeline of the three-way pipe exhausting gas to the outside. When the gas is not discharged to the outside, the third valve can be closed.

[0028] Different from the prior art, in the above technical scheme, bamboo is sliced ​​to obtain bamboo green and bamboo yellow; the bamboo green part of the bamboo is placed in the furnace of the oxygen-free carbonization furnace, natural gas is ignited in the furnace inside the furnace body outside the furnace of the oxygen-free carbonization furnace, and the pyrolysis gas in the furnace containing bamboo yellow is pyrolyzed to 260℃-280℃, and the pyrolysis gas in the furnace is introduced into the condensation tower; the condensation tower discharges the pyrolysis gas below 260℃ to the outside, and introduces the gas above 260℃ into the furnace to spontaneously ignite to form a pyrolysis gas cycle, and cuts off the natural gas; the pyrolysis gas in the furnace containing bamboo yellow is controlled to pyrolyze for 40-90 minutes to obtain high-strength bamboo charcoal carbonized material. The above technical scheme realizes the slicing and utilization of bamboo, and the recycling of the heat energy contained in the combustible gas generated after the pyrolysis of bamboo, so as to obtain high-strength bamboo charcoal.

[0029] The above-mentioned records related to the content of the invention are only an overview of the technical solution of the present invention. In order to enable ordinary technicians in the field to more clearly understand the technical solution of the present invention, and then implement it according to the text of the specification and the contents recorded in the drawings, and in order to make the above-mentioned purpose and other purposes, features and advantages of the present invention easier to understand, the following is a description in combination with the specific implementation mode of the present invention and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The drawings are only used to illustrate the principles, implementations, applications, features and effects of the specific embodiments of the present invention and other related contents, and shall not be considered as limiting the present invention.

[0031] In the drawings of the specification:

[0032] Figure 1 This is a schematic diagram of a bamboo activated carbon production device according to a specific embodiment of the present invention.

[0033] Reference numerals:

[0034] 1. Oxygen-free carbonization furnace;

[0035] 11. Furnace body;

[0036] 12. Furnace;

[0037] 13. Furnace;

[0038] 14. Smoke exhaust pipe;

[0039] 15. The third valve;

[0040] 2. Condensation tower;

[0041] 3. The first valve;

[0042] 4. Second valve;

[0043] 5. The first air outlet;

[0044] 6. The first conveying port;

[0045] 7. Second delivery port;

[0046] 8. First air inlet;

[0047] 9. Tee pipe;

[0048] 10. Burner. DETAILED DESCRIPTION

[0049] In order to explain in detail the possible application scenarios, technical principles, specific schemes that can be implemented, and the purposes and effects of the present invention, the following is a detailed description in combination with the specific embodiments listed and the accompanying drawings. The embodiments described herein are only used to more clearly illustrate the technical solutions of the present invention, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present invention.

[0050] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present invention. The word "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present invention, as long as there is no technical contradiction or conflict, the various technical features mentioned in each embodiment can be combined in any way to form a corresponding implementable technical solution.

[0051] Unless otherwise defined, the technical terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs; the use of relevant terms herein is only for describing specific embodiments and is not intended to limit the present invention.

[0052] In the description of the present invention, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in a logical relationship of "or".

[0053] In the present invention, terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.

[0054] Without further restrictions, in the present invention, the words "include", "comprises", "has" or other similar open-ended expressions used in sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.

[0055] Similar to the understanding in the Examination Guidelines, in the present invention, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of the present invention, the meaning of "multiple" is more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.

[0056] In the description of the embodiments of the present invention, the space-related expressions used, such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "vertical", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicate the orientation or position relationship based on the orientation or position relationship shown in the specific embodiments or drawings, and are only for the convenience of describing the specific embodiments of the present invention or facilitating the reader's understanding, and do not indicate or imply that the referred device or component must have a specific position, a specific orientation, or be constructed or operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present invention.

[0057] Unless otherwise expressly specified or limited, in the description of the embodiments of the present invention, the terms such as "install", "connect", "connect", "fix", "set" and the like used should be understood in a broad sense. For example, the "connection" can be a fixed connection, a detachable connection, or an integrated setting; it can be a mechanical connection, an electrical connection, or a communication connection; it can be a direct connection, or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. For those skilled in the art of the technical field to which the present invention belongs, the specific meanings of the above terms in the embodiments of the present invention can be understood according to the specific circumstances.

[0058] Bamboo charcoal has a long history, but bamboo activated carbon has only been developed in the past two or three decades. Due to the poor strength and high ash content of bamboo activated carbon, the application of this new material activated carbon has not made a breakthrough in the market and technology. The strength and ash content of bamboo activated carbon depend on the control of the bamboo species, origin, age, location, carbonization process, activation process, yield, etc. The hard surface layer of bamboo is bamboo green, and the thick but soft layer inside is bamboo yellow. The whole bamboo is connected by many bamboo nodes.

[0059] At present, there are many applications of activated carbon. The preparation of activated carbon is generally based on coal, fruit shells, and charcoal as the main raw materials. Bamboo activated carbon is a new material. Bamboo is widely available and low-priced, making it an excellent material for making activated carbon. However, due to the limitations of the process and the characteristics of bamboo itself, bamboo activated carbon has a high ash content and poor strength, which is subject to many restrictions in practical applications.

[0060] The components in bamboo are divided into organic matter, inorganic matter and water. The process of carbon making is to convert the oxygen and hydrogen in the organic matter, leaving carbon and inorganic matter in the end. Because the mass of inorganic matter is constant, it will eventually remain in the activated carbon in the form of ash. Therefore, the amount of carbon loss in the carbon making process determines the proportion of ash. If the carbon loss is too large and the proportion of inorganic matter in the raw materials is high, the ash proportion of the final activated carbon will be higher.

[0061] The process of preparing activated carbon is divided into two steps: firing and carbonization, and activation. Firing will convert bamboo into charcoal, but it only has micropores, without the macropores and mesopores of activated carbon. In addition, the micropores are not well developed, and the pore structure is not connected. Activation uses a certain process to fully open and connect the pores of the carbon, thus turning it into activated carbon. The strength of the activated carbon finally produced is a very important indicator. If the strength is not enough, the activated carbon will be shattered during actual use. For example, in the water treatment industry, water must be adsorbed and filtered through activated carbon. If the strength of the activated carbon is not enough, it will be washed after passing through the activated carbon, and the activated carbon will be shattered and flow out with the water, causing black water to appear.

[0062] The carbonization process for preparing activated carbon is divided into aerobic carbonization process and anaerobic carbonization process. At present, the aerobic process is relatively mature, and the mechanical automation degree is high. However, the aerobic process will cause large carbon loss and low yield (high cost), and the ash content of the activated carbon produced is very high and the strength is very poor. The activated carbon carbonized material obtained by the anaerobic process has a higher yield and a lower ash content. However, the anaerobic carbonization process is currently immature, has hidden safety hazards in production, prominent environmental protection issues, poor sealing, and easy blockage of flue gas ducts, and has not yet become mainstream.

[0063] my country is a major producer of activated carbon, but most of it produces low-end activated carbon, which can only be sold for low-end industrial applications with low requirements for ash content and strength, or processed into columnar activated carbon (to avoid strength issues) for use in waste gas treatment.

[0064] To solve the above problems, in a first aspect, the present invention provides a method for preparing bamboo activated carbon, the method comprising:

[0065] The bamboo is sliced ​​to obtain bamboo green and bamboo yellow;

[0066] The green part of bamboo is placed in the furnace of an oxygen-free carbonization furnace, natural gas is ignited in the furnace inside the furnace body outside the furnace of the oxygen-free carbonization furnace, and the pyrolysis gas in the furnace containing the yellow bamboo is pyrolyzed to 260°C-280°C, and the pyrolysis gas in the furnace is introduced into a condensation tower;

[0067] The condensation tower discharges the pyrolysis gas below 260℃ to the outside. If the bamboo vinegar liquid is not collected, the valve should be switched to discharge steam before entering the condensation tower, and the gas above 260℃ should be introduced into the furnace for spontaneous combustion to form a pyrolysis gas cycle, and the natural gas should be cut off;

[0068] The green bamboo part is controlled to be pyrolyzed in the furnace for 40-90 minutes to obtain high-strength bamboo charcoal carbonized material.

[0069] In some embodiments, controlling the pyrolysis of the green bamboo part in the furnace for 40-90 minutes further comprises:

[0070] During the pyrolysis of the green bamboo part, the temperature of the furnace is controlled within the range of 500-650°C.

[0071] To make high-strength bamboo activated carbon, it is necessary to select the green part of bamboo, that is, the green and yellow parts of bamboo slices need to be sliced ​​and carbonized using an anaerobic carbonization process. The carbonization time and temperature need to be controlled (500-650 degrees within 3 hours), and the volatile matter should also be controlled at more than 18%. When activating the carbonized bamboo charcoal, the steam pressure needs to be controlled at 0.03-0.08MPA. The steam needs to use a targeted process to pierce and expand the holes of activated carbon, making full use of the combustion of volatile matter and reducing carbon loss.

[0072] In some embodiments, the method comprises:

[0073] The yellow part of bamboo is placed in the furnace of an oxygen-free carbonization furnace, natural gas is ignited in the furnace area of ​​the furnace body outside the furnace of the oxygen-free carbonization furnace, and the pyrolysis gas in the furnace containing the yellow bamboo is pyrolyzed to 260° C.-280° C., and the pyrolysis gas in the furnace is introduced into a condensation tower;

[0074] The condensation tower condenses the pyrolysis gas below 260°C to collect the bamboo vinegar liquid or discharge it directly to the outside. If the bamboo vinegar liquid is not collected, the valve should be switched to discharge steam before entering the condensation tower, and the gas above 260°C should be introduced into the furnace area to form a pyrolysis gas circulation, and the natural gas should be cut off;

[0075] The bamboo yellow part is controlled to be pyrolyzed in the furnace for 40-60 minutes to obtain low-ash bamboo charcoal carbonized material.

[0076] In some embodiments, controlling the pyrolysis of the bamboo yellow part in the furnace for 40-60 minutes further comprises:

[0077] During the pyrolysis process of the bamboo yellow part, the temperature of the furnace is controlled within the range of 500-550°C.

[0078] To make low-ash activated carbon, it is necessary to select the yellow part of bamboo and remove the bamboo node part, that is, the bamboo node needs to be cut, and the green and yellow bamboo pieces of bamboo need to be sliced, and carbonized using an anaerobic carbonization process. The carbonization time and temperature need to be controlled (500-550 degrees within 2.5 hours), and the volatile matter must also be controlled at more than 15%. When activating the carbonized bamboo charcoal, the steam pressure needs to be controlled at 0.02-0.05MPA. The steam puncture and pore expansion of the activated carbon requires the use of a targeted process to fully utilize the combustion of volatile matter and reduce carbon loss.

[0079] The above method has mastered the control of bamboo activated carbon ash content and strength, and solved the current problems of poor strength and high ash content of bamboo activated carbon. For example, the national standard for bamboo activated carbon ash content is iodine value>400 and ash content less than 15%. With the new process, the iodine value can be>1200, the ash content can be <3%, and even about 1%. At the current stage of the process, the strength of bamboo activated carbon is about 70-85%, and the new process can reach 93-99%.

[0080] See also Figure 1 In the second aspect, the present invention provides an activated carbon production device, which is suitable for the method described in the first aspect, and the production device includes an oxygen-free carbonization furnace 1, a condensation tower 2, a three-way pipe 9 and a valve group;

[0081] The oxygen-free carbonization furnace 1 comprises a furnace body 11, a furnace 12 and a furnace 13. The furnace 12 and the furnace 13 are both arranged in the furnace body 11. The furnace 13 is arranged between the furnace 12 and the furnace body 11. A first air outlet 5 is provided above the furnace 12. A first air inlet 8 is provided on the side wall of the furnace body 11. The first air inlet 8 is communicated with the furnace 13.

[0082] A burner 10, wherein the burner 10 is disposed in the furnace 13, and the first air inlet 8 is disposed on one side of the burner;

[0083] The condensation tower 2 includes a first delivery port 6 and a second delivery port 7, wherein the first delivery port 6 is connected to the first air outlet 5, and the second delivery port 7 is connected to the first air inlet 8;

[0084] The three-way pipe 9 is arranged at the connection point between the first gas outlet 5 and the first delivery port 6, and the other end of the three-way pipe 9 is connected to the outside;

[0085] The valve group includes a first valve 3, a second valve 4 and a third valve 15. The first valve 3 is arranged at the connection between the second delivery port 7 and the first air inlet 8, and the second valve 4 is arranged at the connection between the three-way pipe 9 and the outside. The third valve 15 is placed on the pipeline connecting the three-way pipe 9 and the outside.

[0086] In this embodiment, the first air inlet 8 is arranged through the side wall of the furnace body 11; the burner 10 is used to provide heat energy.

[0087] The burner 10 has two stages. In the first stage, natural gas or other combustible gases are used as fuel for combustion. In the second stage, pyrolysis combustible gas is used as fuel for combustion. At this time, natural gas is turned off and combustion is carried out by pyrolysis gas. Therefore, the first air inlet 8 needs to be connected to the cooling tower 2 to provide sufficient pyrolysis combustible gas.

[0088] It should be further explained that the first air inlet 8, the first air outlet 5, the first delivery port 6 and the second delivery port 7 in this embodiment can be through holes and communicated with each other through pipelines, or can be tubes penetrating the wall, and the tubes are also communicated with each other through pipelines.

[0089] When bamboo vinegar needs to be collected, the third valve 15 can be closed so that the pyrolysis gas can enter the cooling tower through the three-way pipe 9.

[0090] In this embodiment, the oxygen-free carbonization furnace 1 has a furnace body 11, a furnace core 12 and a furnace chamber 13. The furnace chamber 13 is arranged between the furnace core 12 and the furnace body 11 (that is, the furnace chamber 13 covers the furnace core 12). The furnace chamber 13 can be filled with ignited natural gas so that the natural gas can fully pyrolyze the green or yellow bamboo parts in the furnace body 11. The first air inlet 8 and the first air outlet 5 are arranged according to the air flow direction, wherein the first air inlet 8 is arranged on the side of the furnace 13, and the first air outlet 5 is arranged on the top of the furnace 12, then the pyrolysis gas in the bamboo pyrolysis process will be transported from the first air outlet 5 to the condensation tower 2, and there is a distinction between whether to collect bamboo vinegar liquid in this process, when it is necessary to collect bamboo vinegar liquid, the second valve 4 is closed, and the pyrolysis gas condenses the bamboo vinegar liquid through the condensation tower 2, and then the remaining gas below 260°C is discharged to the outside, and the gas above 260°C is re-introduced into the furnace 13, when it is not necessary to collect bamboo vinegar liquid, the second valve 4 is opened, and the pyrolysis gas below 260°C containing bamboo vinegar liquid is discharged before the condensation tower 2, and the remaining pyrolysis gas above 260°C is introduced into the furnace 13. Then it is input from the furnace 13 into the furnace 12 to achieve full anaerobic pyrolysis of bamboo. It should be noted that the process of inputting heat from the furnace 13 into the furnace 12 involves a heat exchange process, and the furnace 13 and the furnace 12 are not connected.

[0091] In this embodiment, the oxygen-free carbonization furnace further includes a smoke exhaust pipe 14, which is disposed at the smoke exhaust port of the furnace body. The smoke exhaust pipe 14 is used to exhaust the sintering smoke. In some embodiments, the smoke is also subjected to environmental protection treatment.

[0092] The corresponding experimental data of the bamboo charcoal carbonized material prepared by the above scheme are as follows:

[0093] Table 1: Carbonized bamboo charcoal from green bamboo parts prepared by the method of this technical solution

[0094]

[0095] Table 2: Carbonized bamboo charcoal from the yellow part of bamboo prepared by the method of this technical solution

[0096]

[0097] Table 3: Bamboo charcoal carbonized material prepared by prior art

[0098]

[0099] It can be seen that compared with the data in Table 1, the strength of the bamboo charcoal carbonized material prepared by the method shown in the present technical solution is significantly improved; compared with the data in Table 2, the ash content of the bamboo charcoal carbonized material prepared by the method shown in the present technical solution is significantly reduced.

[0100] In the above technical scheme, bamboo is sliced ​​to obtain bamboo green and bamboo yellow; the bamboo green part of the bamboo is placed in the furnace of an oxygen-free carbonization furnace, natural gas is ignited in the furnace inside the furnace body outside the furnace of the oxygen-free carbonization furnace, and the pyrolysis gas in the furnace containing bamboo yellow is pyrolyzed to 260°C-280°C, and the pyrolysis gas in the furnace is introduced into a condensation tower; the condensation tower discharges the pyrolysis gas below 260°C to the outside, and introduces the gas above 260°C into the furnace for spontaneous combustion to form a pyrolysis gas cycle, and cuts off the natural gas; the bamboo green part is controlled to pyrolyze in the furnace for 40-90 minutes to obtain a high-strength bamboo charcoal carbonized material. The above technical scheme realizes the slicing and utilization of bamboo, and the recycling of the heat energy contained in the combustible gas generated after the pyrolysis of bamboo, thereby obtaining a high-strength bamboo charcoal carbonized material.

[0101] Finally, it should be noted that although the above embodiments have been described in the specification and drawings of the present invention, the patent protection scope of the present invention cannot be limited thereby. All technical solutions generated by replacing or modifying equivalent structures or equivalent processes based on the essential concept of the present invention and using the contents recorded in the specification and drawings of the present invention, as well as directly or indirectly implementing the technical solutions of the above embodiments in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for producing bamboo activated carbon, characterized in that: The method comprises: The bamboo is sliced ​​to obtain bamboo green and bamboo yellow; The green part of bamboo is placed in the furnace of an oxygen-free carbonization furnace, natural gas is ignited in the furnace inside the furnace body outside the furnace of the oxygen-free carbonization furnace, and the bottom of the furnace containing the green bamboo is heated until the temperature of the pyrolysis gas in the furnace reaches 260°C-280°C; If the temperature of the pyrolysis gas is less than 260° C., the pyrolysis gas is directly discharged to the outside, and / or is discharged to the outside after being collected by the bamboo vinegar liquid in the condensation tower; If the pyrolysis gas is discharged directly to the outside, the valve should be switched to discharge steam outside before entering the condensation tower; If the temperature of the pyrolysis gas is greater than or equal to 260°C, the pyrolysis gas is introduced into the furnace through the condensation tower for spontaneous combustion to form a pyrolysis gas cycle, and the natural gas is cut off; The green bamboo part is controlled to be pyrolyzed in the furnace for 40-90 minutes to obtain high-strength bamboo charcoal carbonized material.

2. The method for producing bamboo activated carbon according to claim 1, characterized in that: Controlling the pyrolysis of the green bamboo part in the furnace for 40-90 minutes also includes: During the pyrolysis process of the green bamboo part, the temperature in the furnace is controlled within the range of 500-650°C.

3. The method for producing bamboo activated carbon according to claim 1, characterized in that: The method comprises: The bamboo yellow part of the bamboo is placed in the furnace of the oxygen-free carbonization furnace, and natural gas is ignited in the furnace area inside the furnace body outside the furnace of the oxygen-free carbonization furnace to heat the bottom of the furnace containing the bamboo yellow until the temperature of the pyrolysis gas in the furnace reaches 260°C-280°C; If the temperature of the pyrolysis gas is less than 260° C., the pyrolysis gas is directly discharged to the outside, and / or is discharged to the outside after being collected by the bamboo vinegar liquid in the condensation tower; If the pyrolysis gas is discharged directly to the outside, the valve should be switched to discharge steam outside before entering the condensation tower; If the temperature of the pyrolysis gas is greater than or equal to 260°C, the pyrolysis gas is introduced into the furnace through the condensation tower for spontaneous combustion to form a pyrolysis gas cycle, and the natural gas is cut off; The green bamboo part is controlled to be pyrolyzed in the furnace for 40-90 minutes to obtain high-strength bamboo charcoal carbonized material. The bamboo yellow part is controlled to be pyrolyzed in the furnace for 40-60 minutes to obtain low-ash bamboo charcoal carbonized material.

4. The method for producing bamboo activated carbon according to claim 3, characterized in that: Controlling the pyrolysis of bamboo yellow in the furnace for 40-60 minutes also includes: The temperature of bamboo yellow pyrolysis in the furnace is in the range of 500-550℃.

5. A bamboo activated carbon production device, characterized in that: The method according to any one of claims 1 to 4, wherein the manufacturing device comprises: An oxygen-free carbonization furnace comprises a furnace body, a furnace core and a furnace chamber, wherein the space between the outside of the furnace core and the inside of the furnace body is a combustion space, namely, the furnace chamber, the furnace core is provided with a first air outlet above, the side wall of the furnace body is provided with a first air inlet, and the first air inlet is connected to the furnace chamber; A burner, the burner is placed at the bottom of the furnace and is used to heat the furnace; A condensation tower, comprising a first delivery port and a second delivery port, wherein the first delivery port is connected to the first air outlet, and the second delivery port is connected to the first air inlet; A three-way pipe is arranged at the connection point between the first gas outlet and the first delivery port, and the other end of the three-way pipe is connected to the outside; The valve group includes a first valve, a second valve and a third valve. The first valve is arranged at the connection between the second delivery port and the first air inlet, the second valve is arranged at the connection between the three-way pipe and the first delivery port; and the third valve is placed on the pipeline connecting the three-way pipe with the outside.