Preparation method of multi-modified SiOX-based negative electrode material based on optimized topological arrangement

By optimizing the preparation method of multi-modified SiOx-based anode material with topological arrangement, Si-Li2Si2O5@C composite material was formed, which solved the problems of low efficiency and cycle performance attenuation of SiOx-based anode material for the first time, and realized the preparation of high-performance anode materials. Meet the application needs of lithium-ion batteries.

CN118908221APending Publication Date: 2024-11-08QINGHAI UNIV OF SCI & TECH (UNDER PREPARATION)
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410880924.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

SiOx-based anode material has problems with low efficiency and attenuation of cycling performance in lithium-ion batteries for the first time, especially poor stability during homogenization under water system conditions, resulting in mechanical stress and electrical contact failure.

Method used

The preparation method of optimized topological arrangement of multiple modified SiOx base negative electrode materials is adopted, and the active lithiide and SiOx powder are premixed by high-energy ball mill to form a topological arrangement structure, and heated and carbon and hydrogen gas deposition in the rotary furnace to form Si-Li2Si2O5@C The composite material removes some of Li2SiO3 and Li4SiO4 to form a core-shell structure with a porous cavity structure.

Benefits of technology

It improves the first Coulomb efficiency and cycle stability of the material, avoids capacity attenuation, and realizes stable homogenization and high-performance negative electrode materials under water system conditions, meeting the application needs of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908221A_ABST
    Figure CN118908221A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a multi-modified SiOx-based negative electrode material based on optimization of topological arrangement, and the method comprises the following steps: carrying out topological arrangement optimization on a Si-SiO2 topological network structure of nano / micro-nano SiOx particles through an active lithium compound reaction to obtain a primary modified Si-Li4SiO4 / Li2SiO3 / Li2Si2O5 topological network structure; the preparation method comprises the following steps: preparing Si-Li2SiO4 / Li2SiO3 / Li2Si2O5 composite particles, performing high-temperature vapor deposition to realize surface carbon deposition coating of the Si-Li4SiO4 / Li2SiO3 / Li2Si2O5 composite particles, and washing with deionized water to remove Li2SiO3 / Li4SiO4 which is easy to dissolve in water, thereby finally obtaining the Si-Li2Si2O5-coated C composite material. The obtained composite material slurry is good in stability, has no gel or sedimentation phenomenon, has high initial coulombic efficiency and long cycle stability, can be prepared in a large scale, and meets the application requirements of high-performance negative electrodes in lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and particularly relates to a method for preparing a multi-modified SiO2 battery based on an optimized topological arrangement. x Method for preparing negative electrode material. Background Art

[0002] As an energy storage device, lithium-ion batteries have been widely used in transportation, electronic communications, wearable devices and other industries. In the research of high energy density negative electrode materials, graphite negative electrode materials have shown superior performance. Therefore, seeking new alternative products has become a challenge for researchers. At present, among all potential alternative products, SiO x SiO-based anode materials are considered to be one of the most competitive anode materials due to their superior capacity performance (1965 mAh / g) and more stable cycle performance compared to single-crystal Si. x It is not composed of a single phase, but is composed of many uniformly distributed nanoscale Si clusters, SiO2 clusters, and SiO transition phases between the Si / SiO2 two-phase interface, forming a topological structure. Therefore, its lithium storage mechanism is very complex. x During the first lithiation process, the product formed is Li x Si, lithium silicate and Li2O, among which Li2O and lithium silicate phases are inert phases, which consume the electrolyte and Li released from the positive electrode. + , and this process is irreversible, resulting in a serious loss of the first reversible capacity, thus leading to a low first coulombic efficiency. Although the presence of O atoms will generate an inert buffer matrix phase in situ, the overall volume effect is still large, and the mechanical stress generated will cause the active material to pulverize and cause electrical contact failure between the current collector; in addition, SiO x The intrinsic conductivity of SiO is low, which is not conducive to the electrochemical performance of the material. Due to the combined influence of the above factors, it eventually leads to x The cycle performance of the negative electrode material is seriously degraded. x Negative electrode materials have great advantages, but there are still many problems in achieving practical application. The most prominent problems are severe capacity attenuation and low first coulombic efficiency.

[0003] In order to improve the first coulombic efficiency of SiOx-based negative electrode materials and improve the long-cycle performance of materials, researchers have taken a variety of modification measures. Pre-lithiation technology can embed lithium into silicon dioxide SiO in advance. xThe material forms lithium silicate, which avoids the consumption of active lithium in the positive electrode and effectively improves the first coulomb efficiency of silicon oxide. However, Li4SiO4 formed by the negative electrode material in the prior art is easily soluble in water, and Li2SiO3 is slightly soluble in water, which has a great impact on the stability of the material, and will cause the pH of the aqueous slurry to increase, and at the same time will produce a large number of bubbles, making the homogenization and coating process extremely difficult.

[0004] Chinese patent document CN111900368A discloses a SiO negative electrode material, which is obtained by mixing SiO with a lithium source and reacting at 300-700°C to obtain pre-lithiated SiO, and then the pre-lithiated SiO is vapor-deposited and carbon-coated in a rotary kiln to obtain a pre-lithiated SiO / C composite material. Finally, it is evenly mixed with a metal oxide and coated on the surface of the composite material. In the pre-lithiation process, this patent can regulate the type and amount of lithium source to increase the proportion of Li2Si2O5 and reduce the generation of Li2SiO3 and Li4SiO4. In addition, in order to inhibit the precipitation and sedimentation of silicates, a layer of metal oxide is coated on the surface of the material, which is of great help to improve the stability of the battery slurry. However, in this patent, the proportion of Li2Si2O5 is regulated only by the type and amount of lithium source, but the water-insoluble Li2Si2O5 and the water-soluble Li2SiO3 are completely mixed. In the silicon-oxygen material, Li2SiO3 is still exposed on the surface of the silicon-oxygen material, which will lead to a higher pH value during the material homogenization process. Therefore, it is necessary to develop a multi-modified SiO x The basic negative electrode material has both high first coulombic efficiency and cycle stability and can be smoothly homogenized under aqueous conditions, which is an urgent problem to be solved in this field. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a multi-modified SiO based on optimized topological arrangement in view of the shortcomings of the prior art. x The invention discloses a method for preparing a negative electrode material, which effectively improves the initial coulombic efficiency of the battery material and improves the long-term cycle stability.

[0006] In order to solve the technical problem of the present invention, the following technical solution is adopted: A multi-modified SiO based on optimized topological arrangement x The method for preparing the base negative electrode material comprises the following steps: (1) Active lithium compounds, SiO x The powders are premixed using a high energy ball mill in an inert gas environment, wherein the mixing ratio is a Li / Si molar ratio of 0.2-0.9:1; (2) heating the mixed material obtained in step (1) in an inert gas environment in a rotary kiln to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999%, the flow rate of the inert gas is 2-6 L / min, the heating temperature is 550-950° C., and the heating time is 0.5-2 h; (3) The material obtained in step (2) is further heated in a rotary kiln and hydrocarbon gas is introduced, wherein the flow ratio of inert gas to hydrocarbon gas is 1:0.5-4, the deposition temperature is 950°C-1100°C, and the deposition time is 1-4h; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, thereby removing part of Li2SiO3 and Li4SiO4 generated in the topological arrangement structure, and after drying, a Si-Li2Si2O5@C composite material with a topological structure is obtained.

[0007] The active lithium compound in step (1) is one of LiH, lithium powder, Li3N and lithium borohydride.

[0008] In step (3), the hydrocarbon gas is one of methane, ethylene and acetylene.

[0009] The inert gas in step (1) and step (2) is argon.

[0010] The rotation speed of the high energy ball mill is 170-260r / min, and the ball-to-material ratio is 2-8:1.

[0011] Compared with the prior art, the present invention has the advantages of SiO x After multiple modifications of the base negative electrode material, the composite material slurry obtained has good stability, no gel or sedimentation phenomenon occurs, and the multiple modified SiO x The material forms a well-ordered topological structure phase due to high-temperature induced lithiation. The pre-formation of this topological structure phase improves the material's initial coulombic efficiency and cycle stability, and can be prepared on a large scale to meet the application requirements for high-performance negative electrodes in lithium-ion batteries.

[0012] The present invention is mainly based on a two-step modification optimization process: the first modification is based on high temperature induced active lithium salt and SiO x The SiO2 in the material reacts to form a topologically arranged active phase of Si and an inactive buffer phase of Li4SiO4 / Li2SiO3 / Li2Si2O5. The topological arrangement of Si and Li4SiO4 / Li2SiO3 / Li2Si2O5 phases was optimized based on the chemical process of high temperature induced dehydrogenation of active lithium salts to drive the lithiation reaction. xThe performance of the material can be attributed to the effective regulation of the well-adjusted Si active phase and the topological arrangement of the inactive phase mainly composed of Li2Si2O5. The inactive phase effectively inhibits the volume expansion of the composite material. Its secondary modification is to coat a layer of carbon shell on the surface of the Si active phase and a small amount of Li4SiO4, a small amount of Li2SiO3 and the main Li2Si2O5 through high-temperature vapor deposition technology, which improves the conductivity of the composite material on the one hand and achieves secondary inhibition of the expansion stress of the composite material on the other hand. The coated material is then washed with deionized water to remove the soluble inert small amount of Li4SiO4 and a small amount of Li2SiO3 inactive buffer phase, forming a composite material with a core-shell structure with a porous cavity. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a schematic diagram of the topological structure of the sample obtained in Example 3 of the present invention; Figure 2 This is the SEM image of the Si-Li2Si2O5@C composite material sample of the present invention; Figure 3 This is a charge and discharge curve diagram of a button-type lithium-ion battery at 1C, in which the sample obtained in Example 3 of the present invention is used as the negative electrode sheet, 1M LiPF6 (DMC:EC=1:1 vol%) +10% FEC is used as the electrolyte, and a polypropylene film is used as the separator. DETAILED DESCRIPTION

[0014] In order to more clearly illustrate the technical solution of the present invention, further description will be given below in conjunction with various embodiments. It should be understood that the implementation of the present invention is not limited to the following embodiments, and any formal modifications and / or changes made to the present invention will fall within the scope of protection of the present invention. In the following embodiments, unless otherwise specified, all percentages are weight units, and the equipment and raw materials used, etc. can be purchased from the market or are commonly used in this area. The methods in the following embodiments, unless otherwise specified, are conventional methods in this area.

[0015] Example 1 A multi-modified SiO based on optimized topological arrangement x The method for preparing the base negative electrode material comprises the following steps: (1) LiH, SiO x The powders were pre-mixed in an argon atmosphere using a high-energy ball mill; the mixing ratio was a Li / Si molar ratio of 0.2:1; the high-energy ball mill speed was 170 r / min, and the ball-to-material ratio was 2:1; (2) heating the mixed material obtained in step (1) in an inert gas argon environment in a rotary furnace to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999% argon, wherein the flow rate of the inert gas is 2 L / min, the heating temperature is 550° C., and the heating time is 0.5 h; (3) The material obtained in step (2) is further heated in a rotary furnace and methane gas is introduced, wherein the flow ratio of high-purity argon gas to methane gas is 1:0.5, the deposition temperature is 950°C, and the deposition time is 1 hour; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, thereby removing part of the Li2SiO3 and Li4SiO4 generated in the topological arrangement structure; after drying, a Si-Li2Si2O5@C composite material with a topological structure is obtained.

[0016] Example 2 A multi-modified SiO based on optimized topological arrangement x The method for preparing the base negative electrode material comprises the following steps: (1) Li3N, SiO x The powders were pre-mixed in an argon atmosphere using a high-energy ball mill; the mixing ratio was a Li / Si molar ratio of 0.9:1; the high-energy ball mill speed was 180 r / min, and the ball-to-material ratio was 3:1; (2) heating the mixed material obtained in step (1) in an inert gas argon environment in a rotary furnace to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999% argon, the flow rate of the inert gas is 3 L / min, the heating temperature is 850° C., and the heating time is 1 h; (3) The material obtained in step (2) is further heated in a rotary furnace and acetylene gas is introduced, with a high-purity argon gas: acetylene gas flow ratio of 1.5:1, a deposition temperature of 1100°C, and a deposition time of 2 hours; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, thereby removing part of the Li2SiO3 and Li4SiO4 generated in the topological arrangement structure; after drying, a Si-Li2Si2O5@C composite material with a topological structure is obtained.

[0017] Example 3 A multi-modified SiO based on optimized topological arrangement x The method for preparing the base negative electrode material comprises the following steps: (1) Lithium borohydride, SiO x The powders were pre-mixed in an argon atmosphere using a high-energy ball mill; the mixing ratio was a Li / Si molar ratio of 0.8:1; the high-energy ball mill speed was 200 r / min, and the ball-to-material ratio was 4:1; (2) heating the mixed material obtained in step (1) in an inert gas argon environment in a rotary furnace to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999% argon, the flow rate of the inert gas is 4 L / min, the heating temperature is 950° C., and the heating time is 2 h; (3) The material obtained in step (2) is further heated in a rotary furnace, and ethylene gas is introduced, with a high-purity argon gas:ethylene gas flow ratio of 1:1, the deposition temperature is 1100°C, and the deposition time is 4 hours; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, thereby removing part of the Li2SiO3 and Li4SiO4 generated in the topological arrangement structure; after drying, a Si-Li2Si2O5@C composite material with a topological structure is obtained.

[0018] Example 4 A multi-modified SiO based on optimized topological arrangement x The method for preparing the base negative electrode material comprises the following steps: (1) Lithium powder, SiO x The powders were pre-mixed in an argon atmosphere using a high-energy ball mill; the mixing ratio was a Li / Si molar ratio of 0.5:1; the high-energy ball mill speed was 210 r / min, and the ball-to-material ratio was 5:1; (2) heating the mixed material obtained in step (1) in an inert gas argon environment in a rotary furnace to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999% argon, the flow rate of the inert gas is 2 L / min, the heating temperature is 550° C., and the heating time is 1 h; (3) The material obtained in step (2) is further heated in a rotary furnace and acetylene gas is introduced, with a flow ratio of high-purity argon gas to acetylene gas of 2:0.5, a deposition temperature of 1000°C, and a deposition time of 2 hours; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, and then dried to obtain a Si-Li2Si2O5@C composite material with a topological structure.

[0019] Example 5 A multi-modified SiO based on optimized topological arrangement x The method for preparing the base negative electrode material comprises the following steps: (1) LiH, SiO x The powders were pre-mixed in an argon atmosphere using a high-energy ball mill; the mixing ratio was a Li / Si molar ratio of 0.9:1; the high-energy ball mill speed was 260 r / min, and the ball-to-material ratio was 5:1; (2) heating the mixed material obtained in step (1) in an inert gas argon environment in a rotary furnace to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999% argon, the flow rate of the inert gas is 6 L / min, the heating temperature is 750° C., and the heating time is 1 h; (3) The material obtained in step (2) is further heated in a rotary furnace and acetylene gas is introduced, with a high-purity argon gas: acetylene gas flow ratio of 2:1, a deposition temperature of 1100°C, and a deposition time of 2 hours; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, thereby removing part of the Li2SiO3 and Li4SiO4 generated in the topological arrangement structure; after drying, a Si-Li2Si2O5@C composite material with a topological structure is obtained.

[0020] Example 6 A multi-modified SiO based on optimized topological arrangement x The method for preparing the base negative electrode material comprises the following steps: (1) Lithium borohydride, SiO x The powders were pre-mixed in an argon atmosphere using a high-energy ball mill; the mixing ratio was a Li / Si molar ratio of 0.5:1; the high-energy ball mill speed was 250 r / min, and the ball-to-material ratio was 8:1; (2) heating the mixed material obtained in step (1) in an inert gas argon environment in a rotary furnace to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999% argon, the flow rate of the inert gas is 5 L / min, the heating temperature is 750° C., and the heating time is 2 h; (3) The material obtained in step (2) is further heated in a rotary furnace, and ethylene gas is introduced, with a high-purity argon gas:ethylene gas flow ratio of 2:1, the deposition temperature is 1100°C, and the deposition time is 1h; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, thereby removing part of the Li2SiO3 and Li4SiO4 generated in the topological arrangement structure; after drying, a Si-Li2Si2O5@C composite material with a topological structure is obtained.

[0021] like Figure 1 As shown, the preparation method of the present invention obtains a material composed of active Si phase and inactive Li4SiO4 / Li2Si2O5, the inactive layer is a single buffer layer of active Si, and a small amount of soluble inert Li4SiO4 and a small amount of Li2SiO3 inactive buffer phase are removed to form a material with a porous cavity structure. The carbon layer structure is coated by vapor deposition technology to form a double buffer layer of active Si, and the two buffer layers are combined to form a composite material with a porous cavity core-shell structure with topological structure arrangement. Figure 2 As shown, the samples obtained by the present invention can be seen through SEM to have different pore structures in the material structure. This is the structure obtained by removing some Li2SiO3 and Li4SiO4 generated in the topological arrangement structure. This structure shortens the transmission distance of ions on the one hand, and provides a good buffer space for the volume expansion of silicon materials on the other hand. Figure 3As shown, the obtained product is used as a negative electrode sheet. From the charge and discharge curve, it can be seen that the first coulomb efficiency of the obtained composite material is 91.6%. Under 1C charge and discharge conditions, the specific capacity after 500 cycles is as high as 600mAh / g.

[0022] The button cell test was performed on the products obtained in Examples 1-6: the Si-Li2Si2O5@C composite material, conductive carbon black, CMC, and SBR prepared in the above-mentioned embodiments were mixed evenly in a ratio of 94:1.5:2:2.5, and applied on copper foil. The coated electrode was placed in a vacuum drying oven at 80°C for vacuum drying for 6 hours for standby use. The simulated battery was assembled in a hydrogen-filled German Braun glove box. The electrolyte was 1MLiPF6+EC:DEC:DMC=1:1:1 (volume ratio). The metal lithium sheet was the counter electrode. The electrochemical performance test was performed on a Wuhan Blue Electric Battery Tester. The charge and discharge voltage range was 0.005V to 2V, and the charge and discharge rate was 0.5C. The test data is shown in Table 1 below: The data in Table 1 show that the Si-Li2Si2O5@C material obtained by the present invention has a high first coulombic efficiency and discharge specific capacity, especially the discharge specific capacity of Example 3 is as high as 1680.3mAh / g, and the first coulombic efficiency is 91.6%. The present invention improves the first coulombic efficiency and cycle stability of the material, and the excellent performance is due to the formation of the optimized topological structure phase and the results of multiple modifications, which can meet the application requirements of high-performance negative electrodes in lithium-ion batteries.

[0023] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. The protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A multi-modified SiO based on optimized topological arrangement x A method for preparing a negative electrode material, characterized in that The steps include: (1) Active lithium compounds, SiO x The powders are premixed using a high energy ball mill in an inert gas environment, wherein the mixing ratio is a Li / Si molar ratio of 0.2-0.9:1; (2) heating the mixed material obtained in step (1) in an inert gas environment in a rotary kiln to react the material to form a topological arrangement structure, wherein the purity of the inert gas is ≥99.999%, the flow rate of the inert gas is 2-6 L / min, the heating temperature is 550-950° C., and the heating time is 0.5-2 h; (3) The material obtained in step (2) is further heated in a rotary kiln and hydrocarbon gas is introduced, wherein the flow ratio of inert gas to hydrocarbon gas is 1:0.5-4, the deposition temperature is 950°C-1100°C, and the deposition time is 1-4h; (4) The material obtained in step (3) is washed with deionized water until the solution is neutral, and part of Li2SiO3 and Li4SiO4 generated in the topological arrangement structure is removed. After drying, a Si-Li2Si2O5@C composite material with a topological structure is obtained.

2. According to claim 1, a multi-modified SiO based on optimized topological arrangement x The method for preparing a base negative electrode material is characterized by: The active lithium compound in step (1) is one of LiH, lithium powder, Li3N and lithium borohydride.

3. According to claim 1 or 2, a multi-modified SiO based on optimized topological arrangement x The method for preparing a base negative electrode material is characterized by: In step (3), the hydrocarbon gas is one of methane, ethylene and acetylene.

4. According to claim 1 or 2, a multi-modified SiO based on optimized topological arrangement x The method for preparing a base negative electrode material is characterized by: The inert gas in step (1) and step (2) is argon.

5. According to claim 4, a method for preparing a multi-modified SiO2 based on an optimized topological arrangement x The method for preparing a base negative electrode material is characterized by: The rotation speed of the high energy ball mill is 170-260r / min, and the ball-to-material ratio is 2-8:1.

Citation Information

Patent Citations

  • Preparation method and application of simple pre-lithiated nano-microstructure silicon-oxygen-carbon composite material

    CN117558894A

  • Negative electrode material and preparation method therefor, and lithium ion battery