Preparation method of layered oxide positive electrode material of sodium-ion battery

In the preparation of sodium ion battery layered oxide positive electrode material, the heating rate is adjusted and the insulation platform is added to ensure that the sodium ions are fully diffused inside the material, solving the problem of residual alkali during sintering, and improving the cycle stability and electricity of the battery Chemical properties.

CN118908307APending Publication Date: 2024-11-08NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411003608.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The residual alkali produced by the layered oxide positive electrode material of sodium ion battery during sintering affects the battery performance, resulting in the material being easily powdered, peeled off, gas-producing bulge and irreversible capacity loss, affecting the battery safety and electrochemical performance.

Method used

By stirring the mixture of sodium, nickel, manganese sources and citric acid at high temperature, forming a precursor, and heating and calcining step by step after ball milling, adjusting the heating rate and adding an insulation platform to ensure that the sodium ions fully diffuse inside the material and reducing material surface residues Alkaline content.

Benefits of technology

The residual alkali content on the surface of the positive electrode material is significantly reduced, the cycle stability and electrochemical performance are improved, the preparation cost of high electrochemical performance materials is reduced, and the cycle stability and capacity retention rate of sodium ion batteries are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908307A_ABST
    Figure CN118908307A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a layered oxide positive electrode material of a sodium ion battery, which comprises the following steps: (1) mixing a sodium source, a nickel source, a manganese source and citric acid in deionized water, continuously stirring to a gel state at high temperature, and then drying to obtain a precursor; and (2) carrying out ball milling on the dried precursor, putting the precursor into a muffle furnace after ball milling, and heating and calcining step by step to obtain the P2-phase Na < 0.67 > Ni < 0.33 > Mn < 0.67 > O2 sodium ion battery layered oxide positive electrode material. According to the method, the residual alkali amount on the surface of the prepared positive electrode material can be reduced, so that the cycling stability of the material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a layered oxide positive electrode material for a sodium ion battery. Background Art

[0002] With the increasing depletion of fossil energy and the continuous growth of energy demand, the development of clean and sustainable new energy is of great significance to human society. At present, the application of lithium-ion batteries has become relatively mature and widespread. Due to its high energy density, it has been widely used in electric vehicles, portable electronic devices and other fields. However, due to the low reserves of lithium resources in the earth's crust, most of them are distributed in South America, which limits the development of lithium-ion batteries, as well as the development of electric vehicles and large-scale energy storage. Therefore, it is necessary to find a substitute for lithium-ion batteries. Sodium-ion batteries have similar "rocking chair" charging and discharging mechanisms and material production equipment as lithium-ion batteries, and sodium resources are abundant and widely distributed. The price of sodium metal is about 1 / 20 of the price of lithium metal. Therefore, the sodium-ion energy storage system has received much attention from scientific research and industry in recent years. In addition, sodium-ion batteries also have good power characteristics, wide temperature range adaptability and high safety, which can be used as a beneficial supplement to lithium-ion batteries.

[0003] Layered oxide cathode materials for sodium ion batteries are considered to have the most promising application prospects due to their high theoretical capacity and high operating voltage platform. However, they also have unavoidable disadvantages. The Na volatilized during the sintering process + Deposited on the surface of the material, it will react with water and carbon dioxide in the air when exposed to the air, and produce substances such as sodium hydroxide, sodium carbonate and sodium bicarbonate on the surface of the material. The above substances are collectively referred to as residual alkali. The residual alkali on the surface of the positive electrode material of the sodium ion battery has many hazards and will affect the battery performance in many aspects. First, the residual alkali is easy to absorb moisture during the battery production process, causing the material to easily form jelly gel during the stirring process, and the electrode is easy to powder and peel off after drying, affecting the processing performance of the positive electrode material; second, the residual sodium carbonate is easy to decompose in the battery system, which will cause the battery to produce gas and bulge, affecting the safety of the battery; third, the alkaline slurry will corrode the aluminum current collector, affecting the transmission of electrons, and the residual alkali compounds will also cause irreversible capacity loss and deteriorate the electrochemical performance of the battery. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a layered oxide positive electrode material for a sodium ion battery. The positive electrode material prepared by this method has a low residual alkali content on the surface, thereby effectively improving the cycle stability performance of the sodium ion battery.

[0005] Technical solution: The method for preparing the layered oxide positive electrode material for sodium ion batteries of the present invention comprises the following steps:

[0006] (1) mixing a sodium source, a nickel source, a manganese source and citric acid in deionized water, stirring continuously at high temperature until a gel state is formed, and then drying the mixture to obtain a precursor;

[0007] (2) The dried precursor is ball-milled, placed in a muffle furnace, and calcined in steps to obtain the P2 phase Na 0.67 Ni 0.33 Mn 0.67 O2 sodium-ion battery layered oxide cathode materials.

[0008] Wherein, in step (1), the sodium source is one of sodium acetate, sodium carbonate or sodium sulfate; the nickel source is one of nickel carbonate, nickel nitrate, nickel acetate or nickel sulfate; the manganese source is one of manganese carbonate, manganese acetate or manganese sulfate.

[0009] Wherein, in step (1), the mixing molar ratio of the sodium source, the nickel source, the manganese source and the citric acid is 0.67:0.33:0.67:1.5.

[0010] Wherein, in step (1), the reaction temperature is 60°C to 80°C; the stirring rate is 500r / min to 2000r / min; and the reaction time is 4h to 6h.

[0011] Wherein, in step (2), the ball-milling bead to precursor ratio is 5:1; the rotation speed of the ball mill is 30-35 r / min, and the ball milling time is 2 h; the dried precursor is ball milled to crush and mix, and the purpose of crushing and mixing is to crush the dried precursor into fine powder, and to perform secondary mixing on the dry matter that is not mixed evenly in the solution, so as to better diffuse the ions during the calcination process.

[0012] Wherein, in step (3), stepwise heating means: heating from room temperature to 400°C, then from 400°C to 500-700°C, keeping at 500-700°C for 2-4h, and finally heating from 500-700°C to 920°C; or heating from room temperature to not less than 400°C, keeping at this temperature for 2-4h, and then heating from this temperature to 920°C. Adding a heat preservation platform during the calcination process is conducive to better crystallization and growth of the material at this temperature.

[0013] Among them, the heating rate from room temperature to 400°C is 3°C / min; the heating rate from 400°C to 500-700°C is 1.5-2°C / min; the heating rate from 500-700°C to 920°C is 1.5-2°C / min.

[0014] The heating rate from room temperature to not less than 400°C is 3°C / min; the heating rate from this temperature to 920°C is 1.5-2°C / min.

[0015] Among them, the holding time after heating to 920°C is 8h to 20h.

[0016] Wherein, in step (3), after heating and calcining, the product is naturally cooled and then collected through a 300-mesh sieve.

[0017] By adjusting the heating rate and adding a heat preservation platform to sinter the positive electrode material through the calcination mechanism, the sodium ions can diffuse more fully and evenly inside the material, thereby reducing the accumulation of sodium ions on the surface of the material and reducing the content of residual alkali on the surface of the material.

[0018] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the method of the present invention can reduce the amount of residual alkali on the surface of the prepared positive electrode material, thereby greatly improving the cycle stability of the material; the method of the present invention can reduce the residual alkali on the surface of the material from the sintering source, thereby eliminating the need for additional doping, coating and modification to reduce the residual alkali, thereby reducing the preparation cost of high electrochemical performance materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a schematic diagram of the calcination mechanism of the present invention;

[0020] Figure 2 Thermogravimetric analysis of P2 material prepared by sol-gel method;

[0021] Figure 3 is the XRD pattern of the positive electrode material in Comparative Example 1;

[0022] Figure 4 The first cycle charge and discharge curves of the positive electrode materials in Comparative Example 1 and Examples 1 to 5 at 0.1C in the voltage range of 2.0V to 4.25V;

[0023] Figure 5 The cycle curves of the positive electrode materials in Comparative Example 1 and Example 1 at 3C in the voltage range of 2.0V to 4.25V;

[0024] Figure 6 The cycle curves of the positive electrode materials in Examples 1, 2, and 3 at 3C in the voltage range of 2.0V to 4.25V;

[0025] Figure 7 The cycle curves of the positive electrode materials in Examples 1, 4 and 5 at 3C in the voltage range of 2.0V to 4.25V;

[0026] Figure 8 GITT comparison diagram of the positive electrode materials in Comparative Example 1 and Example 3;

[0027] Fig. 9 It is a comparison chart of the residual alkali reduction rate of Examples 1 to 5 compared with Comparative Example 1. DETAILED DESCRIPTION

[0028] Example 1

[0029] The method for preparing the layered oxide positive electrode material for sodium ion batteries of the present invention comprises the following steps:

[0030] (1) 5.36 mmol of sodium acetate, 2.64 mmol of nickel acetate and 5.36 mmol of manganese acetate were dissolved in 50 mL of deionized water; 12 mmol of citric acid was dissolved in 50 mL of deionized water, and stirred at a stirring rate of 800 r / min for 20 minutes. After the citric acid was completely dissolved, the citric acid solution was added to the metal salt solution, and the reaction was continued in a 70° C. water bath with continuous stirring until a gel state was obtained, and then dried at 80° C. for 12 hours to obtain a precursor;

[0031] (2) adding the precursor to the ball milling beads, and constantly rotating the ball mill to grind and pulverize the precursor, wherein the ball-to-material ratio of the ball milling beads to the precursor is 5:1; the speed of the ball mill is 30 r / min, and the ball milling time is 2 h;

[0032] (3) The ball-milled sample was placed in an alumina crucible and solid-phase sintered in a muffle furnace. The temperature was first raised from room temperature to 400°C at a heating rate of 3°C / min, then from 400°C to 920°C at a heating rate of 1.5°C / min, and the reaction was kept at 920°C for 12 hours. After natural cooling, the sample was collected through a 300-mesh sieve to obtain P2 phase Na 0.67 Ni 0.33 Mn 0.67 O2 sodium ion positive electrode material.

[0033] Example 2

[0034] The method for preparing the layered oxide positive electrode material for sodium ion batteries of the present invention comprises the following steps:

[0035] (1) 5.36 mmol of sodium acetate, 2.64 mmol of nickel acetate and 5.36 mmol of manganese acetate were dissolved in 50 mL of deionized water; 12 mmol of citric acid was dissolved in 50 mL of deionized water, and stirred at a stirring rate of 800 r / min for 20 minutes. After the citric acid was completely dissolved, the citric acid solution was added to the metal salt solution, and the reaction was continued in a 70° C. water bath with continuous stirring until a gel state was obtained, and then dried at 80° C. for 12 hours to obtain a precursor;

[0036] (2) adding the precursor to the ball milling beads, and constantly rotating the ball mill to grind and pulverize the precursor, wherein the ball-to-material ratio of the ball milling beads to the precursor is 5:1; the speed of the ball mill is 30 r / min, and the ball milling time is 2 h;

[0037] (3) The ball-milled sample was placed in an alumina crucible and solid-phase sintered in a muffle furnace. The temperature was first raised from room temperature to 400°C at a heating rate of 3°C / min and kept at 400°C on a heat preservation platform for 2 hours. The temperature was then raised from 400°C to 920°C at a heating rate of 1.5°C / min and kept at 920°C for 12 hours. After natural cooling, the sample was collected through a 300-mesh sieve to obtain P2 phase Na 0.67 Ni 0.33 Mn 0.67 O2 sodium ion positive electrode material.

[0038] Example 3

[0039] The method for preparing the layered oxide positive electrode material for sodium ion batteries of the present invention comprises the following steps:

[0040] (1) 5.36 mmol of sodium acetate, 2.64 mmol of nickel acetate and 5.36 mmol of manganese acetate were dissolved in 50 mL of deionized water; 12 mmol of citric acid was dissolved in 50 mL of deionized water, and stirred at a stirring rate of 800 r / min for 20 minutes. After the citric acid was completely dissolved, the citric acid solution was added to the metal salt solution, and the reaction was continued in a 70° C. water bath with continuous stirring until a gel state was obtained, and then dried at 80° C. for 12 hours to obtain a precursor;

[0041] (2) adding the precursor to the ball milling beads, and constantly rotating the ball mill to grind and pulverize the precursor, wherein the ball-to-material ratio of the ball milling beads to the precursor is 5:1; the speed of the ball mill is 30 r / min, and the ball milling time is 2 h;

[0042] (3) The ball-milled sample was placed in an alumina crucible and solid-phase sintered in a muffle furnace. The temperature was first raised from room temperature to 400°C at a heating rate of 3°C / min, then raised from 400°C to 500°C at a heating rate of 1.5°C / min, and kept at 500°C on a heat preservation platform for 2 hours; then raised from 500°C to 920°C at a heating rate of 1.5°C / min, and kept at 920°C for 12 hours; after natural cooling, the sample was collected through a 300-mesh sieve to obtain P2 phase Na 0.67 Ni 0.33 Mn 0.67 O2 sodium ion positive electrode material.

[0043] Example 4

[0044] The method for preparing the layered oxide positive electrode material for sodium ion batteries of the present invention comprises the following steps:

[0045] (1) 5.36 mmol of sodium acetate, 2.64 mmol of nickel acetate and 5.36 mmol of manganese acetate were dissolved in 50 mL of deionized water; 12 mmol of citric acid was dissolved in 50 mL of deionized water, and stirred at a stirring rate of 800 r / min for 20 minutes. After the citric acid was completely dissolved, the citric acid solution was added to the metal salt solution, and the reaction was continued in a 70° C. water bath with continuous stirring until a gel state was obtained, and then dried at 80° C. for 12 hours to obtain a precursor;

[0046] (2) adding the precursor to the ball milling beads, and constantly rotating the ball mill to grind and pulverize the precursor, wherein the ball-to-material ratio of the ball milling beads to the precursor is 5:1; the speed of the ball mill is 30 r / min, and the ball milling time is 2 h;

[0047] (3) The ball-milled sample was placed in an alumina crucible and solid-phase sintered in a muffle furnace. The temperature was first raised from room temperature to 400°C at a heating rate of 3°C / min, then raised from 400°C to 600°C at a heating rate of 1.5°C / min, and kept at 600°C on a heat preservation platform for 2 hours; then raised from 600°C to 920°C at a heating rate of 1.5°C / min, and kept at 920°C for 12 hours; after natural cooling, the sample was collected through a 300-mesh sieve to obtain P2 phase Na 0.67 Ni 0.33 Mn 0.67 O2 sodium ion positive electrode material.

[0048] Example 5

[0049] The method for preparing the layered oxide positive electrode material for sodium ion batteries of the present invention comprises the following steps:

[0050] (1) 5.36 mmol of sodium acetate, 2.64 mmol of nickel acetate and 5.36 mmol of manganese acetate were dissolved in 50 mL of deionized water; 12 mmol of citric acid was dissolved in 50 mL of deionized water, and stirred at a stirring rate of 800 r / min for 20 minutes. After the citric acid was completely dissolved, the citric acid solution was added to the metal salt solution, and the reaction was continued in a 70° C. water bath with continuous stirring until a gel state was obtained, and then dried at 80° C. for 12 hours to obtain a precursor;

[0051] (2) adding the precursor to the ball milling beads, and constantly rotating the ball mill to grind and pulverize the precursor, wherein the ball-to-material ratio of the ball milling beads to the precursor is 5:1; the speed of the ball mill is 30 r / min, and the ball milling time is 2 h;

[0052] (3) The ball-milled sample was placed in an alumina crucible and solid-phase sintered in a muffle furnace. The temperature was first raised from room temperature to 400°C at a heating rate of 3°C / min, then raised from 400°C to 700°C at a heating rate of 1.5°C / min, and kept at 700°C on a heat preservation platform for 2 hours; then raised from 700°C to 920°C at a heating rate of 1.5°C / min, and kept at 920°C for 12 hours; after natural cooling, the sample was collected through a 300-mesh sieve to obtain P2 phase Na 0.67 Ni 0.33 Mn 0.67 O2 sodium ion positive electrode material.

[0053] Comparative Example 1

[0054] A method for preparing a layered oxide positive electrode material for a sodium ion battery comprises the following steps:

[0055] (1) 5.36 mmol of sodium acetate, 2.64 mmol of nickel acetate and 5.36 mmol of manganese acetate were dissolved in 50 mL of deionized water; 12 mmol of citric acid was dissolved in 50 mL of deionized water, and stirred at a stirring rate of 800 r / min for 20 minutes. After the citric acid was completely dissolved, the citric acid solution was added to the metal salt solution, and the reaction was continued in a 70° C. water bath with continuous stirring until a gel state was obtained, and then dried at 80° C. for 12 hours to obtain a precursor;

[0056] (2) adding the precursor to the ball milling beads, and constantly rotating the ball mill to grind and pulverize the precursor, wherein the ball-to-material ratio of the ball milling beads to the precursor is 5:1; the speed of the ball mill is 30 r / min, and the ball milling time is 2 h;

[0057] (3) The ball-milled sample was placed in an alumina crucible and solid-phase sintered in a muffle furnace. The temperature was raised from room temperature to 920°C at a heating rate of 3°C / min and kept at 920°C for 12 hours. After natural cooling, the sample was collected through a 300-mesh sieve to obtain P2 phase Na 0.67 Ni 0.33 Mn 0.67 O2 sodium ion positive electrode material.

[0058] The sodium ion positive electrode materials obtained in Examples 1 to 5 and Comparative Example 1 were assembled and tested for button batteries, and the operation was as follows: the positive electrode material was dried at 120°C for 12 hours, and then evenly mixed with a conductive agent and a binder for 4 hours to obtain a slurry, conductive agent: binder: positive electrode material = 10wt%: 10wt%: 80wt%. The prepared slurry was evenly coated on an aluminum foil, and then dried, pressed, and cut into pole pieces, and assembled into button batteries with sodium sheets, glass fiber diaphragms, electrolytes, etc. in an inert atmosphere (such as argon). The assembled button batteries were subjected to capacity tests (2.0V~4.25V, 0.1C / 0.1C) and cycle tests (2.0V~4.25V, 3C / 3C). The results obtained are as follows: Figures 4 to 7 As shown, through Figure 5 It can be seen that by comparing the 3C cycle of Comparative Example 1 and Example 1 in the voltage range of 2.0 to 4.25 V, only reducing the heating rate can improve the cycle performance of the material, and the capacity retention rate is increased from the original 61.3% to 63.5%.

[0059] pass Figure 6 and Figure 7 It can be seen that by comparing Examples 1 to 5 in the voltage range of 2.0 to 4.25 V for 3C cycles, reducing the heating rate and adding a heat preservation platform, Example 3 shows more outstanding performance, with a 3C initial discharge specific capacity close to 90 mAh / g, and a more significant improvement in capacity retention to 72.1%.

[0060] The residual alkali test process is as follows:

[0061] 1. Sample treatment: Take 10g sample and place it in a 250mL beaker, add 90mL pure water, stir magnetically for 20min at a speed of 500r / min, place the turbid liquid in a 30mL centrifuge tube, centrifuge at 8000r / min for 5min, take the upper clear liquid and wait for testing.

[0062] 2. Sodium hydroxide test: first measure 10mL of the upper clear liquid, add 9 drops of titration indicator, which turns blue, and titrate with the calibrated standard acid solution, shaking while dropping until the solution turns bright green, and record the volume of the standard acid solution consumed at the color change point, recorded as V1.

[0063] Substitute into the calculation formula: W NaOH %=V1*C*M1*100 / (m1*1000), wherein C is the molar concentration of the calibrated standard acid solution (C=m*1000 / V / M, m is the mass of anhydrous sodium carbonate, V is the volume of hydrochloric acid consumed, and M1 is the molar mass of anhydrous sodium carbonate), M1 is the molar mass of sodium hydroxide, and m1 is the mass of the corresponding sodium ion battery positive electrode material after high-speed centrifugation of the leachate.

[0064] 3. Sodium carbonate test: first measure 10mL of the upper clear liquid, add 10 drops of titration indicator, which turns blue, and titrate with calibrated standard acid solution, shaking while dropping until the solution turns bright green, record the volume of the standard acid solution consumed at the color change point, recorded as V2, and then continue to titrate until it turns dark red and record the consumed volume as V3.

[0065] Substitute into the calculation formula: W Na2CO3 % = (V3-V2)*C*M2*100 / (m2*1000), wherein C is the molar concentration of the calibrated standard acid solution (C = m*1000 / V / M, m is the mass of anhydrous sodium carbonate, V is the volume of hydrochloric acid consumed, and M is the molar mass of anhydrous sodium carbonate), M2 is the molar mass of sodium carbonate, and m2 is the mass of the corresponding sodium ion battery positive electrode material after high-speed centrifugation of the leachate.

[0066] Table 1 shows the residual alkali test results of the positive electrode materials in Comparative Example 1 and Examples 1 to 5.

[0067] <![CDATA[W NaOH (%)]]> <![CDATA[W Na2CO3 (%)]]> Comparative Example 1 0.264 0.899 Example 1 0.247 0.799 Example 2 0.226 0.759 Example 3 0.196 0.679 Example 4 0.238 0.739 Example 5 0.232 0.742

[0068] It can be seen from the data in Table 1 that the surface residual alkali value of Example 3 is lower, which shows that the calcination mechanism of adjusting the heating rate and adding the insulation platform works, so that the sodium ions are fully and evenly diffused during the formation of the P2 phase, resulting in less accumulation of unevenly dispersed sodium ions on the surface of the material, less reaction with water and carbon dioxide in the air, and the surface residual alkali value is reduced accordingly.

[0069] pass Figure 2 From the thermogravimetric curve, we can see that stage ① is the loss of crystal water in the raw material and the thermal decomposition process of citric acid. When the temperature reaches about 400℃, the crystal water and citric acid in the raw material will decompose. The mass loss in this stage is inevitable. When the corresponding temperature is reached, they will decompose regardless of the heating rate. The slope of stage ② begins to decrease significantly. This process may be that O2 participates in the reaction to generate P2-Na 0.67 Ni 0.33 Mn 0.67 The process of O2, while the slope of stage ③ changes less, which is the growth process of P2 phase. The more important are stages ② and ③, the growth and growth process of P2 phase, which involves the problem of sufficient ion diffusion and structural problems, so the heating rate is reduced and heated slowly to allow the precursor of P2 phase to fully react with oxygen, and to allow the ions in P2 phase to diffuse more fully, and at the same time make the growth of P2 phase more stable.

[0070] By comparing Comparative Example 1 with Example 1, it can be concluded that the slow heating method in stages ② and ③ can improve the cycle performance of the material. By comparing Examples 1 to 5, it can be concluded that under the condition of reducing the heating rate, adding a 500°C insulation platform can not only improve the discharge capacity at a high rate of 3C, but also improve the long cycle stability, and the surface residual alkali value is reduced. This may be because the 500°C insulation platform is the optimal temperature for the decomposition of the precursor. It can be seen from the TG curve that oxygen is involved in stage ②, and the combination with Na also occurs quietly; the thorough decomposition of the precursor is conducive to increasing the contact area with Na reaction, which is convenient for the subsequent heating stage and insulation stage. The layered oxide reacts more gently. Without this insulation platform, the decomposition of the precursor is relatively rapid, local agglomeration will occur, and the subsequent contact reaction with Na will not be thorough, which has an adverse effect on the formation of the material structure.

[0071] Figure 8 It is a GITT comparison diagram of the positive electrode materials in Comparative Example 1 and Example 3; Figure 8 It can be seen that during the battery charging and discharging process, the diffusion rate of sodium ions in the material is improved, indicating that the amount of residual alkali on the surface of the material has decreased, resulting in a decrease in the diffusion resistance of sodium ions in the material.

Claims

1. A method for preparing a layered oxide positive electrode material for a sodium ion battery, characterized in that: The steps include: (1) mixing a sodium source, a nickel source, a manganese source and citric acid in deionized water, stirring continuously at high temperature until a gel state is formed, and then drying the mixture to obtain a precursor; (2) The dried precursor is ball-milled, and then heated and calcined step by step to obtain the P2 phase Na 0.67 Ni 0.33 Mn 0.67 Layered oxide cathode materials for O2 sodium-ion batteries.

2. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step (1), the sodium source is one of sodium acetate, sodium carbonate or sodium sulfate; the nickel source is one of nickel carbonate, nickel nitrate, nickel acetate or nickel sulfate; the manganese source is one of manganese carbonate, manganese acetate or manganese sulfate.

3. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step (1), the mixing molar ratio of the sodium source, the nickel source, the manganese source and the citric acid is 0.67:0.33:0.67:1.5-3.

4. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step (1), the reaction temperature is 60°C to 80°C; the stirring rate is 500r / min to 2000r / min; and the reaction time is 4h to 6h.

5. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step (2), the ball-to-material ratio of ball milling beads to precursor is 5:1-1.5; the rotation speed of the ball mill is 30-35 r / min, and the ball milling time is 2-2.5 h.

6. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 1, characterized in that: In step (3), stepwise heating means: heating from room temperature to 400°C, then heating from 400°C to 500-700°C, keeping at 500-700°C for 2-4h, and finally heating from 500-700°C to 920°C; or heating from room temperature to not less than 400°C, keeping at this temperature for 2-4h, and then heating from this temperature to 920°C.

7. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 6, characterized in that: The heating rate from room temperature to 400°C is 3-3.5°C / min; the heating rate from 400°C to 500-700°C is 1.5-2°C / min; the heating rate from 500-700°C to 920°C is 1.5-2°C / min.

8. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 6, characterized in that: The heating rate from room temperature to not less than 400°C is 3-3.5°C / min; the heating rate from this temperature to 920°C is 1.5-2°C / min.

9. The method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 6, characterized in that: The holding time after heating to 920°C is 8h to 20h.

Citation Information

Cited By

  • Manganese-based layered oxide with mixed structure as well as preparation method and application of manganese-based layered oxide

    CN119683690A