Preparation method of nano-structure double-coated nickel-cobalt-manganese ternary positive electrode material and prepared ternary positive electrode material

By adopting nanostructured double-covering technology on nickel, cobalt, manganese ternary positive electrode material, the inner layer of magnesium, aluminum spinel nanopowder and outer layer of carbon nanotubes, the corrosion problem of the material in the electrolyte is solved and improved Lithium-ion batteries have cycling performance, rate performance and safety performance.

CN118943353AInactive Publication Date: 2024-11-12GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411327878.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The corrosion effect of nickel-cobalt-manganese ternary cathode material in the electrolyte results in capacity decay and affects cycle stability. It is difficult for the prior art to effectively improve its cycle performance, rate performance and safety performance.

Method used

The preparation method of nanostructure double-coated is adopted, the inner layer is coated with magnesium-aluminum spinel nanopowder and the outer layer is coated with carbon nanotubes. A stable coating structure is formed through ball milling and heat treatment to reduce the contact between the material and the electrolyte. Enhance electrical conductivity and structural stability.

Benefits of technology

It significantly improves the circulation performance, rate performance and safety performance of lithium-ion batteries, enhances the structural stability and electronic conductivity of the materials, and improves the safety and high-temperature cycle stability of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943353A_ABST
    Figure CN118943353A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a nano-structure double-coated cobalt-nickel-manganese ternary positive electrode material, and relates to the technical field of nickel-cobalt-manganese ternary positive electrode materials, and the preparation method comprises the following steps: (1) primary coating: weighing a lithium salt, a metal hydroxide precursor and magnesium aluminate spinel nano-powder according to a certain mass ratio, mixing, ball-milling, carrying out heat treatment, washing with water, and drying to obtain a lithium-nickel-manganese ternary positive electrode material; the nickel-cobalt-manganese ternary positive electrode material coated with the magnesium aluminate spinel nano powder is obtained; and (2) secondary coating: weighing the primary coating material and a carbon nano tube according to a certain mass ratio, stirring and mixing in absolute ethyl alcohol, centrifuging, drying and sieving to obtain the magnesium aluminate spinel nano powder and carbon nano tube double-coated nickel-cobalt-manganese ternary positive electrode material. The invention also provides the cobalt-nickel-manganese ternary positive electrode material prepared by the method. The coated nickel-cobalt-manganese ternary positive electrode material has the beneficial effects that the coated nickel-cobalt-manganese ternary positive electrode material is high in structural stability and excellent in conductivity, and a lithium ion battery prepared from the material has excellent cycle performance under high voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nickel-cobalt-manganese ternary positive electrode materials, and in particular to a preparation method of a nanostructured double-coated cobalt-nickel-manganese ternary positive electrode material and the prepared ternary positive electrode material. Background Art

[0002] As energy crisis and environmental pollution become increasingly prominent, it is imperative to develop sustainable new energy and build a low-carbon society. Lithium-ion batteries, as a new type of high-energy green battery, have attracted much attention. Layered nickel-cobalt-manganese ternary cathode material is a material with great development prospects. Compared with LiCoO 2 , LiNiO 2 , and LiMnO 2 , it has the advantages of low cost, large capacity, good cycle performance, good thermal stability, and relatively stable structure.

[0003] Although nickel-cobalt-manganese ternary positive electrode materials have many advantages, there are still some problems with this material, such as the electrolyte has a certain corrosive effect on the electrode material, which causes the capacity of the material to decay and affects the cycle stability of the material. Therefore, the modification of the positive electrode material has become an important means to improve the electrochemical performance of the material, among which coating is the simplest and most effective method. The presence of the coating layer can maintain its own surface structure stability, avoid direct contact between the active material and the electrolyte, and inhibit the dissolution of transition metal elements in the material under high potential conditions, thereby improving the capacity retention rate of the positive electrode material.

[0004] For example, the patent application with publication number CN112803009A discloses coating lithium boron oxide on the surface of primary particles of nickel-cobalt-manganese ternary positive electrode material to form regularly shaped polyhedral particles, inhibiting the generation of microcracks and improving cycle stability. However, the obtained nickel-cobalt-manganese ternary positive electrode material is assembled into a button-type battery, and the capacity retention rate after 100 cycles at a rate of 1C is 92.1%. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a coated nickel-cobalt-manganese ternary positive electrode material and the prepared nickel-cobalt-manganese ternary positive electrode material, which can improve the cycle performance, rate performance and safety performance of the battery.

[0006] The present invention solves the above technical problems through the following technical means: A method for preparing a nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material comprises the following steps: (1) Primary coating: A. ball milling magnesium aluminum spinel nanopowder; B. Ball milling: mixing the lithium salt, the nickel-cobalt-manganese hydroxide precursor, and the magnesium-aluminum spinel nanopowder after ball milling in step (1), and performing dry ball milling. After ball milling, the ball milling beads are separated to obtain a black powder; C. Heat treatment: heat treating the obtained black powder until the reaction is complete to obtain a nickel-cobalt-manganese ternary positive electrode material coated with magnesium-aluminum spinel nanopowder; (2) Secondary coating: The primary coating material, carbon nanotubes and ethanol solution are mixed and stirred, and the mixed solution is centrifuged, dried and sieved to obtain a nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material.

[0007] Beneficial effects: The preparation method of the present invention adopts double-layer coating, the inner layer is coated with magnesium aluminum spinel nanopowder, and the outer layer is coated with carbon nanotubes. Magnesium aluminum spinel nanopowder has the characteristics of high melting point, low thermal expansion coefficient, good abrasion resistance and good chemical stability. Using it as a coating for nickel-cobalt-manganese ternary materials can stabilize the crystal structure of the material on the one hand, and reduce the contact between the nickel-cobalt-manganese ternary positive electrode material matrix and the electrolyte on the other hand, effectively inhibiting the corrosion of trace hydrofluoric acid in the electrolyte and improving the safety of the battery.

[0008] The outer carbon nanotube coating can enhance the conductivity of the material, and the coating can reduce the residual alkali content in the matrix of the ternary positive electrode material, improve the structural stability and electronic conductivity of the material, so the lithium-ion battery made of this positive electrode material has excellent cycle performance, rate performance and safety performance at high voltage.

[0009] The preparation method provided by the invention is simple to operate, has strong feasibility and high safety.

[0010] Preferably, in step A, the magnesium aluminum spinel nanopowder is dry-milled in a ball mill at a rotation speed of 500 to 1000 rpm for 0.5 to 5 hours.

[0011] Preferably, in step B, the ball mill jar is made of polytetrafluoroethylene, the ball mill beads are made of zirconium dioxide, the particle size of the ball mill beads is 5 to 10 mm, the ball mill speed is 200 to 2000 rad / min, and the mass ratio of the ball mill beads to the mixed material is 1:1 to 2.

[0012] Preferably, the preparation method of the nickel-cobalt-manganese hydroxide precursor comprises the following steps: dissolving nickel salt, cobalt salt and manganese salt in water to obtain a mixed salt solution, mixing the mixed solution with an alkaline solution, and adding a complexing agent at the same time; after the reaction is completed, stirring, heating, and introducing an inert gas, and obtaining a nickel-cobalt-manganese hydroxide precursor after aging, filtering, washing, drying, and grinding.

[0013] Preferably, the preparation method of the nickel-cobalt-manganese hydroxide precursor specifically comprises the following steps: dissolving nickel salt, cobalt salt and manganese salt in deionized water to prepare a mixed salt solution of 1-2.5 mol·L-1, and preparing 2-4 mol·L-1 alkaline solution at the same time, inputting the salt solution and the alkaline solution into a reaction container at a flow rate of 1-10 L / min by a peristaltic pump, and adding a certain concentration of complexing agent to the reaction container to mix evenly, adjusting the temperature of the reaction container at 50-60°C, the pH value at 10.9-11.5, the stirring frequency at 18-25 Hz, passing inert gas for not less than 20 minutes, adjusting the flow rate of the alkaline solution to control the pH of the system to remain stable, and after the reaction is completed, continuing to stir, heat and pass inert gas for 4-6 hours, and then aging for 4-20 hours, washing and filtering with deionized water for 3 times, and then drying the obtained precipitate in a blast drying oven at 85-100°C, and grinding to obtain a nickel-cobalt-manganese hydroxide precursor.

[0014] Preferably, the nickel salt, cobalt salt and manganese salt are respectively selected from one or more of sulfates, nitrates and chlorides; the alkali in the alkaline solution is selected from a mixture of one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide; the complexing agent is selected from a mixture of one or more of ammonia water, ammonium sulfate, sodium citrate and iminodiacetic acid.

[0015] Preferably, the lithium salt is one or a combination of at least two of lithium nitrate, lithium acetate, lithium oxalate, lithium chloride, lithium carbonate, and lithium hydroxide, the molar ratio of the lithium salt to the nickel-cobalt-manganese ternary precursor is (1-1.15):1, and the mass ratio of the nickel-cobalt-manganese ternary precursor to the magnesium-aluminum spinel nanopowder is 1000:(10-100).

[0016] Preferably, the stoichiometric ratio of the nickel salt, the cobalt salt and the manganese salt is a:b:c, wherein 0.6≤a≤0.9, 0.1≤b<0.4, 0.1<c<0.4, and a+b+c=1.

[0017] Preferably, the inert gas is selected from one of high-purity nitrogen and argon.

[0018] Preferably, the concentration of the complexing agent is 0.10-0.55 mol / L, and the molar ratio of the added complexing agent to the base is 1:4.

[0019] Preferably, the molar ratio of lithium carbonate to the nickel-cobalt-manganese hydroxide precursor in step B is 1.05:1, and the mass ratio of the nickel-cobalt-manganese hydroxide precursor to the magnesium-aluminum spinel nanopowder after ball milling in step (1) is 1000:10-100.

[0020] Preferably, the temperature raising procedure of the heat treatment in step C is: raising the temperature to 700-1000° C. at a rate of 5-8° C. / min at room temperature, then keeping the temperature for 6 hours and then cooling naturally.

[0021] Preferably, in step (2), the diameter and length of the carbon nanotubes are 1-30 nm and 1-60 μm, respectively.

[0022] Preferably, in step (2), the mass ratio of the primary coating material to the carbon nanotubes is 0.1 to 1:1000.

[0023] Preferably, in step (2), the ratio of the total mass of the primary coating material and the carbon nanotubes to the volume of the ethanol solution is 5-50 g:100 ml.

[0024] Preferably, the primary coating material, carbon nanotubes and ethanol solution in step (2) are stirred at a temperature of 25-60° C. for 15-30 min.

[0025] Preferably, the centrifugal speed in step (2) is 2000-5000 r / min, the number of centrifugation is at least one, the centrifugal time each time is 3-15 min, and the washing solution after centrifugation is one or both of deionized water and anhydrous ethanol.

[0026] Preferably, the mesh size of the sieve used in step (2) is 500 meshes.

[0027] A nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material prepared by the preparation method.

[0028] The advantages of the present invention are as follows: the preparation method of the present invention adopts double-layer coating, the inner layer is coated with magnesium aluminum spinel nano powder, and the outer layer is coated with carbon nano tubes. Magnesium aluminum spinel nano powder has the characteristics of high melting point, low thermal expansion coefficient, good abrasion resistance and good chemical stability. Using it as a coating for nickel-cobalt-manganese ternary material can stabilize the crystal structure of the material on the one hand, and reduce the contact between the nickel-cobalt-manganese ternary positive electrode material matrix and the electrolyte on the other hand, effectively inhibiting the corrosion of trace hydrofluoric acid in the electrolyte and improving the safety of the battery.

[0029] The outer carbon nanotube coating can enhance the conductivity of the material, and the coating can reduce the residual alkali content in the matrix of the ternary positive electrode material, improve the structural stability and electronic conductivity of the material, so the lithium-ion battery made of this positive electrode material has excellent cycle performance, rate performance and safety performance at high voltage.

[0030] The preparation method provided by the invention is simple to operate, has strong feasibility and high safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is an electron microscope image of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material in Example 1 of the present invention; Figure 2High temperature cycle curves of 45°C at a test voltage of 3.0-4.4V for a wound soft-pack battery made of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material in Example 1 of the present invention and a wound soft-pack battery made of the nickel-cobalt-manganese ternary positive electrode material in Comparative Example 3. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0034] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions. Example

[0035] The preparation method of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material specifically comprises the following steps: (1) Preparation of nickel-cobalt-manganese ternary cathode material precursor: Nickel nitrate, cobalt nitrate and manganese nitrate are used as raw materials, weighed according to a stoichiometric ratio (0.7:0.1:0.2) and dissolved in deionized water to prepare a 1 mol·L -1 mixed salt solution, and a 2 mol·L -1 lithium hydroxide aqueous solution is prepared at the same time. The salt solution and the alkaline solution are simultaneously input into a reaction container at a flow rate of 8 L / min through a peristaltic pump, and 0.35 mol / L ammonia water is added to the reaction container to mix evenly, the temperature of the reaction container is adjusted to 55° C., the pH value is 10.9-11.5, the stirring frequency is 18 Hz, an inert gas is introduced for not less than 20 minutes, the flow rate of the alkaline solution is adjusted to control the pH of the system to remain stable, and after the reaction is completed, stirring, heating and inert gas are continued for 4 hours, and then static aging is performed for 8 hours. After washing and suction filtration with deionized water for 3 times, the obtained precipitate is placed in an 85° C. blast drying oven to be fully dried, and a nickel-cobalt-manganese hydroxide precursor is obtained after grinding.

[0036] (2) Primary coating: A. Dry-mill the purchased magnesium aluminum spinel nanopowder in a ball mill at a speed of 800 rpm for 2 h; B. Ball milling and mixing: lithium carbonate and nickel cobalt manganese hydroxide precursor are weighed at a molar ratio of 1.05:1, and the ball-milled magnesium aluminum spinel nanopowder is weighed at a mass ratio of 1000 (nickel cobalt manganese hydroxide precursor): 30, and the powders are added to a ball mill respectively, and dry-milled for 12 hours. After the ball milling, the ball milling beads are separated to obtain a black powder; wherein the ball mill is made of polytetrafluoroethylene, the ball milling beads are made of zirconium dioxide, the particle size of the ball milling beads is 5 mm, the ball milling speed is 200 rad / min, and the mass ratio of the ball milling beads to the mixed material is 1:2; C. Heat treatment: heat-treating the powder obtained in step B until the reaction is completed to obtain a nickel-cobalt-manganese ternary positive electrode material coated with magnesium-aluminum spinel nanopowder, wherein the temperature rise program of the heat treatment is: heating to 850°C at 5°C / min at room temperature, then keeping at this temperature for 6 hours and then cooling naturally; (3) Secondary coating: The primary coating material and carbon nanotubes (tube diameter 20 nm, tube length 45 μm) were weighed at a mass ratio of 0.08:1000, and the weighed primary coating material and carbon nanotubes were mixed with an ethanol solution at a mass volume ratio of 40 g:100 ml, and stirred at 45°C for 20 min to obtain a mixed solution. The obtained mixed solution was centrifuged at 2000 r / min, dried, and passed through a 500-mesh sieve to obtain a nickel-cobalt-manganese ternary positive electrode material double-coated with magnesium-aluminum spinel nanopowder and carbon nanotubes. Example

[0037] The preparation method of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material specifically comprises the following steps: (1) Preparation of nickel-cobalt-manganese ternary cathode material precursor: nickel nitrate, cobalt nitrate and manganese nitrate were used as raw materials, weighed according to the stoichiometric ratio (0.7:0.1:0.2) and dissolved in deionized water to prepare a 1 mol·L-1 mixed salt solution, and a 2 mol·L-1 lithium hydroxide aqueous solution was prepared at the same time. The salt solution and the alkaline solution were simultaneously input into the reaction container at a flow rate of 8 L / min by a peristaltic pump, and 0.35 mol / L ammonia water was added to the reaction container to mix evenly. The temperature of the reaction container was adjusted to 55°C, the pH value was 10.9-11.5, the stirring frequency was 18 Hz, and an inert gas was introduced for not less than 20 minutes. The flow rate of the alkaline solution was adjusted to control the pH of the system to remain stable. After the reaction was completed, stirring, heating and inert gas were continued for 4 hours, and then static aging was performed for 8 hours. After washing and suction filtration with deionized water for 3 times, the obtained precipitate was placed in a blast drying oven at 85°C to be fully dried, and the nickel-cobalt-manganese hydroxide precursor was obtained after grinding; (2) Primary coating: A. Dry-mill the purchased magnesium aluminum spinel nanopowder in a ball mill at a speed of 800 rpm for 2 h; B. Ball milling and mixing: lithium carbonate and nickel cobalt manganese hydroxide precursor are weighed at a molar ratio of 1.05:1, and the ball-milled magnesium aluminum spinel nanopowder is weighed at a mass ratio of 1000 (nickel cobalt manganese hydroxide precursor): 20, and the powders are added to a ball mill respectively, and dry-milled for 12 hours. After the ball milling, the ball milling beads are separated to obtain a black powder; wherein the ball mill is made of polytetrafluoroethylene, the ball milling beads are made of zirconium dioxide, the particle size of the ball milling beads is 10 mm, the ball milling speed is 2000 rad / min, and the mass ratio of the ball milling beads to the mixed material is 1:1; C. Heat treatment: heat-treating the powder obtained in step B until the reaction is completed to obtain a nickel-cobalt-manganese ternary positive electrode material coated with magnesium-aluminum spinel nanopowder, wherein the temperature rise program of the heat treatment is: heating to 850°C at 5°C / min at room temperature, then keeping at this temperature for 6 hours and then cooling naturally; (3) Secondary coating: The primary coating material and carbon nanotubes (tube diameter 20 nm, tube length 45 μm) were weighed at a mass ratio of 0.03:1000, and the weighed primary coating material and carbon nanotubes were mixed with an ethanol solution at a mass volume ratio of 40 g:100 ml, and stirred at 45°C for 20 min to obtain a mixed solution. The obtained mixed solution was centrifuged at 5000 r / min, dried, and passed through a 500-mesh sieve to obtain a nickel-cobalt-manganese ternary positive electrode material double-coated with magnesium-aluminum spinel nanopowder and carbon nanotubes. Example

[0038] The preparation method of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material specifically comprises the following steps: (1) Preparation of nickel-cobalt-manganese ternary cathode material precursor: nickel nitrate, cobalt nitrate and manganese nitrate were used as raw materials, weighed according to the stoichiometric ratio (0.7:0.1:0.2) and dissolved in deionized water to prepare a 1 mol·L-1 mixed salt solution, and 2 mol·L-1 lithium hydroxide was prepared at the same time. The salt solution and the alkaline solution were simultaneously input into the reaction container at a flow rate of 8 L / min by a peristaltic pump, and 0.35 mol / L ammonia water was added to the reaction container to mix evenly. The temperature of the reaction container was adjusted to 55°C, the pH value was 10.9-11.5, the stirring frequency was 18 Hz, and an inert gas was introduced for not less than 20 minutes. The flow rate of the alkaline solution was adjusted to control the pH of the system to remain stable. After the reaction was completed, stirring, heating and inert gas were continued for 4 hours, and then static aging was performed for 8 hours. After washing and suction filtration with deionized water for 3 times, the obtained precipitate was placed in a blast drying oven at 85°C to be fully dried, and the nickel-cobalt-manganese hydroxide precursor was obtained after grinding; (2) Primary coating: A. Dry-mill the purchased magnesium aluminum spinel nanopowder in a ball mill at a speed of 800 rpm for 2 h; B. Ball milling and mixing: lithium carbonate and nickel cobalt manganese hydroxide precursor are weighed at a molar ratio of 1.05:1, and the ball-milled magnesium aluminum spinel nanopowder is weighed at a mass ratio of 1000 (nickel cobalt manganese hydroxide precursor): 60, and the powders are added to a ball mill respectively, and dry-milled for 12 hours. After the ball milling, the ball milling beads are separated to obtain a black powder; wherein the ball mill is made of polytetrafluoroethylene, the ball milling beads are made of zirconium dioxide, the particle size of the ball milling beads is 10 mm, the ball milling speed is 1000 rad / min, and the mass ratio of the ball milling beads to the mixed material is 1:2; C. Heat treatment: heat-treating the powder obtained in step B until the reaction is completed to obtain a nickel-cobalt-manganese ternary positive electrode material coated with magnesium-aluminum spinel nanopowder, wherein the temperature rise program of the heat treatment is: heating to 850°C at 5°C / min at room temperature, then keeping at this temperature for 6 hours and then cooling naturally; (3) Secondary coating: The primary coating material and carbon nanotubes (tube diameter 20 nm, tube length 45 μm) were weighed at a mass ratio of 0.05:1000, and the weighed primary coating material and carbon nanotubes were mixed with an ethanol solution at a mass volume ratio of 40 g:100 ml, and stirred at 45°C for 20 min to obtain a mixed solution. The obtained mixed solution was centrifuged at 2500 r / min, dried, and passed through a 500-mesh sieve to obtain a nickel-cobalt-manganese ternary positive electrode material double-coated with magnesium-aluminum spinel nanopowder and carbon nanotubes. Example

[0039] The preparation method of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material specifically comprises the following steps: (1) Preparation of nickel-cobalt-manganese ternary cathode material precursor: Nickel nitrate, cobalt nitrate and manganese nitrate are used as raw materials, weighed according to a stoichiometric ratio (0.7:0.1:0.2) and dissolved in deionized water to prepare a 2.5 mol·L-1 mixed salt solution, and a 4 mol·L-1 lithium hydroxide aqueous solution is prepared at the same time. The salt solution and the alkaline solution are simultaneously input into a reaction container at a flow rate of 1 L / min through a peristaltic pump, and 0.35 mol / L ammonia water is added to the reaction container to mix evenly, the temperature of the reaction container is adjusted at 60°C, the pH value is 10.9-11.5, the stirring frequency is 25 Hz, an inert gas is introduced for not less than 20 minutes, the flow rate of the alkaline solution is adjusted to control the pH of the system to remain stable, after the reaction is completed, stirring, heating and inert gas are continued for 6 hours, and then static aging is performed for 20 hours. After washing and suction filtration with deionized water for 3 times, the obtained precipitate is placed in a 100°C blast drying oven for full drying, and a nickel-cobalt-manganese hydroxide precursor is obtained after grinding.

[0040] (2) Primary coating: A. Dry-mill the purchased magnesium aluminum spinel nanopowder in a ball mill at a speed of 1000 rpm for 0.5 h; B. Ball milling and mixing: lithium carbonate and nickel cobalt manganese hydroxide precursor are weighed at a molar ratio of 1.05:1, and the ball-milled magnesium aluminum spinel nanopowder is weighed at a mass ratio of 1000 (nickel cobalt manganese hydroxide precursor): 30, and the powders are added to a ball mill respectively, and dry-milled for 12 hours. After the ball milling, the ball milling beads are separated to obtain a black powder; wherein the ball mill is made of polytetrafluoroethylene, the ball milling beads are made of zirconium dioxide, the particle size of the ball milling beads is 5 mm, the ball milling speed is 200 rad / min, and the mass ratio of the ball milling beads to the mixed material is 1:2; C. Heat treatment: heat-treating the powder obtained in step B until the reaction is completed to obtain a nickel-cobalt-manganese ternary positive electrode material coated with magnesium-aluminum spinel nanopowder, wherein the heating program of the heat treatment is: heating at 8°C / min to 1000°C at room temperature, then keeping at this temperature for 6 hours and then cooling naturally; (3) Secondary coating: The primary coating material and carbon nanotubes (tube diameter 20 nm, tube length 45 μm) were weighed at a mass ratio of 0.08:1000, and the weighed primary coating material and carbon nanotubes were mixed with an ethanol solution at a mass volume ratio of 40 g:100 ml, and stirred at 60°C for 15 min to obtain a mixed solution. The obtained mixed solution was centrifuged at 5000 r / min, dried, and passed through a 500-mesh sieve to obtain a nickel-cobalt-manganese ternary positive electrode material double-coated with magnesium-aluminum spinel nanopowder and carbon nanotubes.

[0041] The structure and morphology of the ternary material prepared in this embodiment are different from those in embodiments 1, 2, and 3, but the double coating of the nanostructure can also stabilize the material structure and improve the electrochemical performance of the material (compared with the comparative example). Example

[0042] The preparation method of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material specifically comprises the following steps: (1) Preparation of nickel-cobalt-manganese ternary cathode material precursor: Nickel nitrate, cobalt nitrate and manganese nitrate are used as raw materials, weighed according to a stoichiometric ratio (0.6:0.2:0.2), and then dissolved in deionized water to prepare a 2 mol·L -1 mixed salt solution. At the same time, a 3 mol·L -1 lithium hydroxide aqueous solution is prepared. The salt solution and the alkaline solution are simultaneously input into a reaction container at a flow rate of 10 L / min through a peristaltic pump. At the same time, 0.35 mol / L ammonia water is added to the reaction container and mixed evenly. The temperature of the reaction container is adjusted at 50° C., the pH value is 10.9-11.5, the stirring frequency is 20 Hz, an inert gas is introduced for not less than 20 minutes, the flow rate of the alkaline solution is adjusted to control the pH of the system to remain stable, and after the reaction is completed, stirring, heating and inert gas are continued for 6 hours, and then static aging is performed for 10 hours. After washing and suction filtration with deionized water for 3 times, the obtained precipitate is placed in a 90° C. forced air drying oven for full drying, and the nickel-cobalt-manganese hydroxide precursor is obtained after grinding.

[0043] (2) Primary coating: A. Dry-mill the purchased magnesium aluminum spinel nanopowder in a ball mill at a speed of 500 rpm for 5 h; B. Ball milling and mixing: lithium carbonate and nickel cobalt manganese hydroxide precursor are weighed at a molar ratio of 1.05:1, and the ball-milled magnesium aluminum spinel nanopowder is weighed at a mass ratio of 1000 (nickel cobalt manganese hydroxide precursor): 30, and the powders are added to a ball mill respectively, and dry-milled for 6 hours. After the ball milling, the ball milling beads are separated to obtain a black powder; wherein the ball mill is made of polytetrafluoroethylene, the ball milling beads are made of zirconium dioxide, the particle size of the ball milling beads is 5 mm, the ball milling speed is 200 rad / min, and the mass ratio of the ball milling beads to the mixed material is 1:1; C. Heat treatment: heat-treating the powder obtained in step B until the reaction is completed to obtain a nickel-cobalt-manganese ternary positive electrode material coated with magnesium-aluminum spinel nanopowder, wherein the heating program of the heat treatment is: heating to 700°C at 5°C / min at room temperature, then keeping at this temperature for 6 hours and then cooling naturally; (3) Secondary coating: The primary coating material and carbon nanotubes (tube diameter 20 nm, tube length 45 μm) were weighed at a mass ratio of 0.1:1000, and the weighed primary coating material and carbon nanotubes were mixed with an ethanol solution at a mass volume ratio of 5 g:100 ml, and stirred at 25°C for 30 min to obtain a mixed solution. The obtained mixed solution was centrifuged at 2500 r / min, dried, and passed through a 500-mesh sieve to obtain a nickel-cobalt-manganese ternary positive electrode material double-coated with magnesium-aluminum spinel nanopowder and carbon nanotubes.

[0044] The structure and morphology of the ternary material prepared in this embodiment are different from those in embodiments 1, 2, and 3, but the double coating of the nanostructure can also stabilize the material structure and improve the electrochemical performance of the material (compared with the comparative example).

[0045] Comparative Example 1 Compared with Example 1, this example is different in that the secondary carbon nanotube coating in step (3) is not performed.

[0046] Comparative Example 2 The present embodiment is different from the embodiment 1 in that the surface is only coated with carbon nanotubes, that is, the nickel-cobalt-manganese ternary positive electrode material is directly coated for the second time.

[0047] Comparative Example 3 The present embodiment is different from the embodiment 1 in that the nickel-cobalt-manganese ternary positive electrode material is not coated with any substance.

[0048] The embodiment and the comparative example were matched with the same negative electrode, electrolyte, and separator to prepare a 3Ah wound soft-pack lithium-ion battery of the same specification, but the nickel-cobalt-manganese ternary positive electrode material in the present invention is not limited to the preparation of a 3Ah wound soft-pack lithium-ion battery, and the electrical performance test was carried out under the following test conditions: ① 0.33C charge and discharge test; ② 45℃ high temperature 0.5C / 1C rate cycle test; ③ 25℃ 3C rate discharge test. The test results are shown in Table 1.

[0049] Table 1 is the performance test results of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode materials in each embodiment and comparative example From the comparison of the data in the table, it can be seen that the ternary positive electrode material prepared by the method of the present invention has higher cycle stability, higher energy utilization and rate performance. The magnesium aluminum spinel nanopowder coating layer stabilizes the structure of the material and improves the high temperature cycle stability of the material, but an overly thick coating layer will hinder the diffusion of lithium ions. Therefore, the thickness of the coating layer should be reasonably controlled. The carbon nanotube coating layer improves the ionic conductivity and electronic conductivity of the material, effectively improving the rate performance of the material.

[0050] Figure 1 This is an electron microscope image of the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material in Example 1. It can be seen that the coating effect is good through this method.

[0051] Figure 2 The 45°C high-temperature cycle curves of the wound soft-pack battery made of the ternary Ni65 single crystal positive electrode material coated in Example 1 and the wound soft-pack battery made of the ternary Ni65 single crystal positive electrode material matrix (Comparative Example 3) used in Example 1 at a test voltage of 3.0-4.4V. It can be seen that the 100-week capacity retention rate of the nanostructure double-coating under high voltage is close to 99%, while the 100-week capacity retention rate of the uncoated one is only about 93%, and the capacity decay is serious.

[0052] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material, characterized in that: The following steps are involved: (1) Primary coating: A. ball milling magnesium aluminum spinel nanopowder; B. Ball milling: mixing the lithium salt, the nickel-cobalt-manganese hydroxide precursor, and the magnesium-aluminum spinel nanopowder after ball milling in step (1), and performing dry ball milling. After ball milling, the ball milling beads are separated to obtain a black powder; C. Heat treatment: heat treating the obtained black powder until the reaction is complete to obtain a nickel-cobalt-manganese ternary positive electrode material coated with magnesium-aluminum spinel nanopowder; (2) Secondary coating: The primary coating material, carbon nanotubes and ethanol solution are mixed and stirred, and the mixed solution is centrifuged, dried and sieved to obtain a nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material.

2. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 1, characterized in that: In the step A, the magnesium aluminum spinel nano powder is dry-milled in a ball mill at a rotation speed of 500 to 1000 rpm for 0.5 to 5 hours.

3. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 1, characterized in that: The preparation method of the nickel-cobalt-manganese hydroxide precursor comprises the following steps: dissolving nickel salt, cobalt salt and manganese salt in water to obtain a mixed salt solution, mixing the mixed solution with an alkaline solution, adding a complexing agent, stirring, heating and introducing an inert gas after the reaction is completed, and obtaining the nickel-cobalt-manganese hydroxide precursor after aging, filtering, washing, drying and grinding.

4. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 3, characterized in that: The nickel salt, cobalt salt and manganese salt are respectively selected from one or more of sulfate, nitrate and chloride; the alkali in the alkaline solution is selected from a mixture of one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide; the complexing agent is selected from a mixture of one or more of ammonia water, ammonium sulfate, sodium citrate and iminodiacetic acid.

5. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 1, characterized in that: The lithium salt is one of lithium nitrate, lithium acetate, lithium oxalate, lithium chloride, lithium carbonate, and lithium hydroxide, or a combination of at least two thereof; the molar ratio of the lithium salt to the nickel-cobalt-manganese ternary precursor is (1-1.15):1; the mass ratio of the nickel-cobalt-manganese ternary precursor to the magnesium-aluminum spinel nanopowder is 1000:(10-100).

6. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 1, characterized in that: The molar ratio of lithium carbonate to the nickel-cobalt-manganese hydroxide precursor in step B is 1.05:1, and the mass ratio of the nickel-cobalt-manganese hydroxide precursor to the magnesium-aluminum spinel nanopowder after ball milling in step (1) is 1000:10-100.

7. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 1, characterized in that: The heating procedure of the heat treatment in step C is: heating to 700-1000° C. at 5-8° C. / min at room temperature, then keeping at this temperature for 6 hours and then cooling naturally.

8. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 1, characterized in that: In the step (2), the mass ratio of the primary coating material to the carbon nanotubes is 0.1 to 1:1000.

9. The method for preparing the nanostructured double-coated nickel-cobalt-manganese ternary positive electrode material according to claim 1, characterized in that: In the step (2), the ratio of the total mass of the primary coating material and the carbon nanotubes to the volume of the ethanol solution is 5-50g:100ml.