Nano magnetic flocculant as well as preparation method and application thereof

Through the modification treatment of nanomagnetic flocculants, combined with silica coating and phenylalanine-modified chitosan, the problem of low removal rate of sulfonamide antibiotics in the prior art is solved, and efficient drinking water treatment is achieved. The removal rate reaches 90%.

CN118908378AActive Publication Date: 2024-11-08ANHUI UNIVERSITY OF ARCHITECTURE

Patent Information

Application Number
CN202411009103.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing drinking water treatment process has poor effect on removing sulfonamide antibiotics, and the interaction between existing flocculants and sulfonamide antibiotics is not strong, resulting in a removal rate of less than 60%.

Method used

Using nanomagnetic flocculants, the adsorption performance and stability of the flocculants are improved by combining modified iron tetraoxide nanospheres with silica coating and phenylalanine-modified chitosan, and electrostatic attraction and hydrogen The bonding effect enhances the adsorption effect on sulfonamide antibiotics and achieves efficient removal with magnetic field separation.

Benefits of technology

It realizes efficient removal of trace amounts of sulfonamide antibiotics in drinking water, with a removal rate of 90%, and the preparation method is simple and easy to operate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963783750000081
    Figure BDA0004963783750000081
Patent Text Reader

Abstract

The invention discloses a nano magnetic flocculant and a preparation method and application thereof, and belongs to the technical field of drinking water treatment.The preparation method comprises the following steps that S1, modified ferroferric oxide nanospheres are ultrasonically dispersed in an ammonia water-ethanol solution, tetraethoxysilane is slowly and dropwise added while stirring is conducted, stirring continues after dropwise adding is completed, washing is conducted after centrifugal separation, and a modified ferroferric oxide nanosphere is obtained; the ferroferric oxide nanoparticles coated with silicon dioxide are obtained; s2, phenylalanine modified chitosan is added into a glacial acetic acid solution, after phenylalanine modified chitosan is completely swelled and dissolved, silicon dioxide coated ferroferric oxide nanoparticles are added for ultrasonic treatment and irradiated under a low-pressure ultraviolet lamp, then absolute ethyl alcohol is used for washing and purifying, vacuum drying is conducted till the weight is constant, and a nano magnetic flocculant is obtained; the method disclosed by the invention is simple and easy to operate, and the prepared nano magnetic flocculant can be quickly adsorbed to the surface of the sulfonamide antibiotics to generate a flocculation effect and can be magnetically separated, so that the nano magnetic flocculant is very suitable for efficiently removing trace sulfonamide antibiotics in a drinking water source.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of drinking water treatment, and specifically relates to a nano magnetic flocculant and a preparation method and application thereof. Background Art

[0002] With the development of animal husbandry and aquaculture, the types and usage of antibiotics have increased greatly. Antibiotics can enter the water environment through various pathways after use. In recent years, sulfonamide antibiotics have been detected in drinking water sources in succession and at high concentrations, causing pollution to drinking water and threatening people's health and safety. The conventional treatment process of existing drinking water plants has a relatively good removal effect on macromolecular substances, but it is not targeted at emerging pollutants such as sulfonamide antibiotics, resulting in poor removal of sulfonamide antibiotics. When existing flocculants are used to treat raw water containing trace amounts of sulfonamide antibiotics, it is difficult for antibiotics to form a strong interaction in the flocs, resulting in the treatment efficiency of existing flocculants being limited, with a removal rate of less than 60%. In order to improve the interaction between flocculants and sulfonamide antibiotics, it is necessary to improve existing flocculants. Summary of the invention

[0003] The purpose of the present invention is to provide a nano magnetic flocculant and a preparation method and application thereof, so as to solve the problems in the background technology.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a nano magnetic flocculant comprises the following steps:

[0006] Step S1, ultrasonically dispersing the modified ferroferric oxide nanospheres in an ammonia ethanol solution, slowly dropping ethyl orthosilicate while mechanically stirring, continuing to stir for 24 hours after the dropping is completed, centrifugally separating and washing with distilled water and anhydrous ethanol for several times to obtain silicon dioxide-coated ferroferric oxide nanoparticles;

[0007] Step S2, adding phenylalanine modified chitosan to glacial acetic acid solution, adding silicon dioxide coated ferrosoferric oxide nanoparticles after complete swelling and dissolution, ultrasonic treatment for 10 minutes, irradiating under a low-pressure ultraviolet lamp for 2-3 hours, then washing and purifying with anhydrous ethanol for 6-8 times, and vacuum drying at 60° C. to constant weight to obtain a nano magnetic flocculant.

[0008] Furthermore, the modified ferroferric oxide nanospheres are prepared by the following steps:

[0009] The ferroferric oxide nanoparticles were dispersed in deionized water, and then hydrochloric acid solution and sodium citrate solution were added and stirred for 2-3 hours to modify the surface of the ferroferric oxide nanoparticles, and then magnetically filtered and washed several times with anhydrous ethanol and distilled water to obtain modified ferroferric oxide nanospheres. Sodium citrate was adsorbed on the surface of the ferroferric oxide nanoparticles, changing its surface potential, which was beneficial for the ferroferric oxide nanoparticles to overcome the magnetic dipole moment.

[0010] Furthermore, the dosage ratio of the ferroferric oxide nanoparticles, deionized water, hydrochloric acid solution and sodium citrate solution is 0.15-2g:50mL:10mL:100mL; the concentration of the hydrochloric acid solution is 2mol / L; and the concentration of the sodium citrate solution is 0.5mol / L.

[0011] Furthermore, the usage ratio of the modified ferrosoferric oxide nanospheres, the ammonia ethanol solution and tetraethyl orthosilicate is 0.15-2g:45-46mL:0.45mL; the ammonia ethanol solution is a mixture of 25wt% ammonia and ethanol in a volume ratio of 1:75.

[0012] Furthermore, the phenylalanine-modified chitosan is prepared by the following steps:

[0013] Chitosan was added into hydrochloric acid solution and stirred to dissolve, and then the pH of the solution was adjusted to 5-6. After adding the mixed solution and stirring for 2 hours, phenylalanine solution was added dropwise and reacted at 25°C with magnetic stirring for 4 hours. The reaction product was poured into acetone for precipitation, filtered and washed, and vacuum dried for 24 hours to obtain phenylalanine-modified chitosan.

[0014] Furthermore, the dosage ratio of the chitosan, hydrochloric acid solution, mixed solution and phenylalanine solution is 1g:100mL:18-20mL:100mL; the concentration of the hydrochloric acid solution is 1wt%; and the concentration of the phenylalanine solution is 0.5wt%.

[0015] Furthermore, the mixed solution is obtained by mixing and dissolving 4-dimethylaminopyridine, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N,N-dimethylformamide in a dosage ratio of 0.1-0.2 g: 0.1-0.2 g: 20 mL.

[0016] Furthermore, the usage ratio of the phenylalanine-modified chitosan, the glacial acetic acid solution and the silicon dioxide-coated ferrosoferric oxide nanoparticles is 1.5 g:15 mL:2 g; and the concentration of the glacial acetic acid solution is 1 wt %.

[0017] A nano magnetic flocculant is prepared by the above preparation method.

[0018] Application of a nano-magnetic flocculant in removing trace amounts of sulfonamide antibiotics in drinking water sources comprises the following steps:

[0019] The nano magnetic flocculant is added into the raw water from the drinking water source at a dosage of 10-12 mg / L, stirred and mixed for 5-10 minutes, and then allowed to settle for 2 hours. After the flocculants are separated by magnetic force, the trace sulfonamide antibiotics in the drinking water source are removed.

[0020] Beneficial effects of the present invention:

[0021] The invention uses sodium citrate to modify the surface of ferroferric oxide nanoparticles to obtain modified ferroferric oxide nanospheres, which can not only improve the dispersibility by changing the surface potential, but also help to overcome the magnetic dipole moment; then, by dripping ethyl orthosilicate solution, silicon dioxide-coated ferroferric oxide nanoparticles are prepared; the magnetic ferroferric oxide nanoparticles are coated with silicon dioxide, which can improve the stability of the ferroferric oxide nanoparticles and also improve the adsorption performance to a certain extent; finally, under ultraviolet light irradiation, the silicon dioxide-coated ferroferric oxide nanoparticles are reacted and grafted with phenylalanine-modified chitosan to obtain a nano magnetic flocculant; the phenylalanine group in the phenylalanine-modified chitosan can react with sulfonamide to form a nano magnetic flocculant; Electrostatic attraction, π-electron interaction and hydrogen bonding between antibiotic molecules promote the adsorption bridging and net-catching sweeping effects of the nano-magnetic flocculant, thereby improving the removal effect of sulfonamide antibiotics in drinking water sources; the amino group in the chitosan molecular structure is also easy to combine with the benzene ring in the sulfonamide antibiotic molecules, so the nano-magnetic flocculant of the present invention can be quickly adsorbed to the surface of the sulfonamide antibiotics under the joint promotion of various aspects, and further produce flocculation, and finally can quickly separate flocs under the action of a magnetic field; therefore, the nano-magnetic flocculant of the present invention is very suitable for the efficient removal of trace sulfonamide antibiotics in drinking water sources, with a removal rate of up to 90%, and its preparation method is simple and easy to operate. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] A method for preparing a nano magnetic flocculant comprises the following steps:

[0025] Step S1, dispersing 0.15g of ferroferric oxide nanoparticles into 50mL of deionized water, then adding 10mL of 2mol / L hydrochloric acid solution and 100mL of 0.5mol / L sodium citrate solution, stirring and mixing for 2h, magnetically filtering, and washing with anhydrous ethanol and distilled water for 3 times to obtain modified ferroferric oxide nanospheres;

[0026] Step S2, ultrasonically dispersing 0.15 g of modified ferroferric oxide nanospheres in 45 mL of an ammonia-ethanol solution, wherein the ammonia-ethanol solution is a mixture of 25 wt% ammonia and ethanol in a volume ratio of 1:75, slowly dropping 0.45 mL of ethyl orthosilicate while mechanically stirring, continuing to stir for 24 h after the dropping is complete, centrifugally separating and washing with distilled water and anhydrous ethanol for 3 times to obtain silicon dioxide-coated ferroferric oxide nanoparticles;

[0027] Step S3, adding 1g of chitosan to 100mL of 1wt% hydrochloric acid solution and stirring to dissolve, then adjusting the pH of the solution to 6, adding 18mL of a mixed solution and stirring to react for 2h, wherein the mixed solution is obtained by mixing and dissolving 4-dimethylaminopyridine, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N,N-dimethylformamide in a dosage ratio of 0.1g:0.1g:20mL, adding 100mL of 0.5wt% phenylalanine solution dropwise, reacting for 4h under magnetic stirring at 25°C, pouring the reaction product into acetone for precipitation, filtering and washing, and vacuum drying for 24h to obtain phenylalanine-modified chitosan;

[0028] Step S4, adding 1.5 g of phenylalanine-modified chitosan to 15 mL of 1 wt% glacial acetic acid solution, adding 2 g of silicon dioxide-coated ferrosoferric oxide nanoparticles after complete swelling and dissolution, ultrasonically treating for 10 min, irradiating under a low-pressure ultraviolet lamp for 2 h, then washing and purifying with anhydrous ethanol for 6 times, and vacuum drying at 60° C. to constant weight to obtain a nanomagnetic flocculant.

[0029] Example 2

[0030] A method for preparing a nano magnetic flocculant comprises the following steps:

[0031] Step S1, dispersing 0.18g of ferroferric oxide nanoparticles into 50mL of deionized water, then adding 10mL of 2mol / L hydrochloric acid solution and 100mL of 0.5mol / L sodium citrate solution, stirring and mixing for 2h, magnetically filtering, and washing with anhydrous ethanol and distilled water for 3 times to obtain modified ferroferric oxide nanospheres;

[0032] Step S2, ultrasonically dispersing 0.18 g of modified ferroferric oxide nanospheres in 45 mL of an ammonia-ethanol solution, wherein the ammonia-ethanol solution is a mixture of 25 wt% ammonia and ethanol in a volume ratio of 1:75, slowly dropping 0.45 mL of ethyl orthosilicate while mechanically stirring, continuing to stir for 24 h after the dropping is complete, centrifugally separating and washing with distilled water and anhydrous ethanol for 3 times to obtain silicon dioxide-coated ferroferric oxide nanoparticles;

[0033] Step S3, adding 1g of chitosan to 100mL of 1wt% hydrochloric acid solution and stirring to dissolve, then adjusting the pH of the solution to 5, adding 20mL of a mixed solution and stirring to react for 2h, wherein the mixed solution is obtained by mixing and dissolving 4-dimethylaminopyridine, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N,N-dimethylformamide in a dosage ratio of 0.15g:0.15g:20mL, adding 100mL of 0.5wt% phenylalanine solution dropwise, reacting for 4h under magnetic stirring at 25°C, pouring the reaction product into acetone for precipitation, filtering and washing, and vacuum drying for 24h to obtain phenylalanine-modified chitosan;

[0034] Step S4, adding 1.5 g of phenylalanine-modified chitosan to 15 mL of 1 wt% glacial acetic acid solution, adding 2 g of silicon dioxide-coated ferrosoferric oxide nanoparticles after complete swelling and dissolution, ultrasonically treating for 10 min, irradiating under a low-pressure ultraviolet lamp for 3 h, then washing and purifying with anhydrous ethanol for 7 times, and vacuum drying at 60° C. to constant weight to obtain a nanomagnetic flocculant.

[0035] Example 3

[0036] A method for preparing a nano magnetic flocculant comprises the following steps:

[0037] Step S1, dispersing 2g of ferroferric oxide nanoparticles into 50mL of deionized water, then adding 10mL of 2mol / L hydrochloric acid solution and 100mL of 0.5mol / L sodium citrate solution, stirring and mixing for 3h, magnetically filtering, and washing with anhydrous ethanol and distilled water for 3 times to obtain modified ferroferric oxide nanospheres;

[0038] Step S2, ultrasonically dispersing 2 g of modified ferroferric oxide nanospheres in 46 mL of an ammonia ethanol solution, wherein the ammonia ethanol solution is a mixture of 25 wt% ammonia water and ethanol in a volume ratio of 1:75, slowly dropping 0.45 mL of ethyl orthosilicate while mechanically stirring, continuing to stir for 24 h after the dropping is complete, centrifugally separating and washing with distilled water and anhydrous ethanol for 3 times to obtain silicon dioxide-coated ferroferric oxide nanoparticles;

[0039] Step S3, adding 1g of chitosan to 100mL of 1wt% hydrochloric acid solution and stirring to dissolve, then adjusting the solution pH to 6, adding 20mL of a mixed solution and stirring to react for 2h, wherein the mixed solution is obtained by mixing and dissolving 4-dimethylaminopyridine, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N,N-dimethylformamide in a dosage ratio of 0.2g:0.2g:20mL, adding 100mL of 0.5wt% phenylalanine solution dropwise, reacting for 4h under magnetic stirring at 25°C, pouring the reaction product into acetone for precipitation, filtering and washing, and vacuum drying for 24h to obtain phenylalanine-modified chitosan;

[0040] Step S4, adding 1.5 g of phenylalanine-modified chitosan to 15 mL of 1 wt% glacial acetic acid solution, adding 2 g of silicon dioxide-coated ferrosoferric oxide nanoparticles after complete swelling and dissolution, ultrasonically treating for 10 min, irradiating under a low-pressure ultraviolet lamp for 3 h, then washing and purifying with anhydrous ethanol for 8 times, and vacuum drying at 60° C. to constant weight to obtain a nanomagnetic flocculant.

[0041] Comparative Example 1

[0042] The difference between this comparative example and Example 3 is that the operation of step S2 is not performed, and the modified ferrosoferric oxide nanospheres are not subjected to silicon dioxide coating treatment, and the remaining steps are the same.

[0043] Comparative Example 2

[0044] The difference between this comparative example and Example 3 is that step S3 is not performed, chitosan is not modified with phenylalanine, and the remaining steps are the same.

[0045] Example 4

[0046] This embodiment provides an application of a nano-magnetic flocculant for removing trace amounts of sulfonamide antibiotics in drinking water sources, comprising the following steps:

[0047] The nano magnetic flocculant prepared in Example 1 was added into raw water taken from a drinking water source at a dosage of 10 mg / L, wherein the sulfonamide antibiotic in the raw water was sulfadiazine. After stirring and mixing for 5 minutes, the mixture was allowed to settle for 2 hours. After magnetic separation of the flocs, the trace sulfonamide antibiotics in the drinking water source were removed.

[0048] Example 5

[0049] This embodiment provides an application of a nano-magnetic flocculant for removing trace amounts of sulfonamide antibiotics in drinking water sources, comprising the following steps:

[0050] The nano magnetic flocculant prepared in Example 2 was added into raw water taken from a drinking water source at a dosage of 11 mg / L, wherein the sulfonamide antibiotic in the raw water was sulfadiazine. After stirring and mixing for 8 minutes, the mixture was allowed to settle for 2 hours. After magnetic separation of the flocs, the trace sulfonamide antibiotics in the drinking water source were removed.

[0051] Example 6

[0052] This embodiment provides an application of a nano-magnetic flocculant for removing trace amounts of sulfonamide antibiotics in drinking water sources, comprising the following steps:

[0053] The nano magnetic flocculant prepared in Example 3 was added to raw water taken from a drinking water source at a dosage of 12 mg / L, where the sulfonamide antibiotic in the raw water was sulfadiazine. After stirring and mixing for 10 minutes, the mixture was allowed to settle for 2 hours. After magnetic separation of the flocs, the trace sulfonamide antibiotics in the drinking water source were removed.

[0054] Comparative Example 3

[0055] Compared with Example 6, this comparative example uses an equal amount of commercially available polyaluminium chloride flocculant to replace the nano-magnetic flocculant prepared in Example 3, and the remaining steps are the same.

[0056] Comparative Example 4

[0057] Compared with Example 6, this comparative example uses an equal amount of the nano-magnetic flocculant prepared in Comparative Example 1 to replace the nano-magnetic flocculant prepared in Example 3, and the remaining steps are the same.

[0058] Comparative Example 5

[0059] Compared with Example 6, this comparative example uses an equal amount of the nano-magnetic flocculant prepared in Comparative Example 2 to replace the nano-magnetic flocculant prepared in Example 3, and the remaining steps are the same.

[0060] The concentration of sulfonamide antibiotics in the raw water before and after flocculation treatment of Example 4-Example 6 and Comparative Example 3-Comparative Example 5 was measured by liquid chromatography-mass spectrometry, and the removal rate of sulfonamide antibiotics in each group of treatment was recorded and calculated. The results are shown in Table 1:

[0061] Table 1

[0062]

[0063] It can be seen from the data in Table 1 that the nano magnetic flocculant prepared by the present invention has an excellent removal effect on trace sulfonamide antibiotics in drinking water sources, with a removal rate of more than 90%, showing significant advantages over the existing polyaluminium chloride flocculants; the coating treatment of modified ferroferric oxide nanospheres by silica and the modification of chitosan by phenylalanine can synergistically promote each other, thereby improving the removal effect and efficiency of sulfonamide antibiotics in drinking water sources.

[0064] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a nano magnetic flocculant, It is characterized in that The following steps are involved: Step S1, ultrasonically dispersing the modified ferroferric oxide nanospheres in an ammonia ethanol solution, slowly dropping ethyl orthosilicate while stirring, continuing to stir for 24 hours after the dropping is complete, centrifugally separating and washing with distilled water and anhydrous ethanol for several times to obtain silicon dioxide-coated ferroferric oxide nanoparticles; Step S2, adding phenylalanine modified chitosan to glacial acetic acid solution, adding silicon dioxide coated ferrosoferric oxide nanoparticles after complete swelling and dissolution, ultrasonically treating for 10 minutes, irradiating under a low-pressure ultraviolet lamp for 2-3 hours, then washing and purifying with anhydrous ethanol, and vacuum drying to constant weight to obtain a nano magnetic flocculant.

2. The method for preparing a nano magnetic flocculant according to claim 1, It is characterized in that The modified ferroferric oxide nanospheres are prepared by the following steps: The ferrosoferric oxide nanoparticles are dispersed in deionized water, and then hydrochloric acid solution and sodium citrate solution are added and stirred for 2-3 hours. The mixture is subjected to magnetic filtration and washed with anhydrous ethanol and distilled water to obtain modified ferrosoferric oxide nanospheres.

3. The method for preparing a nano magnetic flocculant according to claim 2, It is characterized in that The dosage ratio of the ferroferric oxide nanoparticles, deionized water, hydrochloric acid solution and sodium citrate solution is 0.15-2g:50mL:10mL:100mL; the concentration of the hydrochloric acid solution is 2mol / L; the concentration of the sodium citrate solution is 0.5mol / L.

4. The method for preparing a nano magnetic flocculant according to claim 1, It is characterized in that The usage ratio of the modified ferrosoferric oxide nanospheres, the ammonia ethanol solution and ethyl orthosilicate is 0.15-2:45-46:0.45 mL; the ammonia ethanol solution is a mixture of 25wt% ammonia and ethanol in a volume ratio of 1:

75.

5. The method for preparing a nano magnetic flocculant according to claim 1, It is characterized in that The phenylalanine modified chitosan is prepared by the following steps: Chitosan was added into hydrochloric acid solution and stirred to dissolve, and then the pH of the solution was adjusted to 5-6. After adding the mixed solution and stirring for 2 hours, phenylalanine solution was added dropwise and reacted at 25°C with magnetic stirring for 4 hours. The reaction product was poured into acetone for precipitation, filtered, washed, and vacuum dried to obtain phenylalanine-modified chitosan.

6. The method for preparing a nano magnetic flocculant according to claim 5, It is characterized in that The dosage ratio of the chitosan, the hydrochloric acid solution, the mixed solution and the phenylalanine solution is 1g:100mL:18-20mL:100mL; the concentration of the hydrochloric acid solution is 1wt%; and the concentration of the phenylalanine solution is 0.5wt%.

7. The method for preparing a nano magnetic flocculant according to claim 6, It is characterized in that The mixed solution is prepared by mixing and dissolving 4-dimethylaminopyridine, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N,N-dimethylformamide in a dosage ratio of 0.1-0.2 g: 0.1-0.2 g: 20 mL.

8. The method for preparing a nano magnetic flocculant according to claim 1, It is characterized in that The dosage ratio of the phenylalanine-modified chitosan, the glacial acetic acid solution and the silicon dioxide-coated ferrosoferric oxide nanoparticles is 1.5 g:15 mL:2 g; and the concentration of the glacial acetic acid solution is 1 wt %.

9. A nano magnetic flocculant, It is characterized in that Prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the nano magnetic flocculant according to claim 9 in removing trace amounts of sulfonamide antibiotics in drinking water sources.

Citation Information

Patent Citations

  • Acid-resistant magnetic chitosan microspheres as well as preparation method and application thereof

    CN104437395A

  • Amino-acid-modified chitosan flocculating agent and preparation method and application thereof

    CN105601764A

  • Preparation of magnetic chitosan composite adsorption material and application in dye wastewater treatment

    CN106582560A

  • Preparation method and application of cationic chitosan-based magnetic flocculant initiated by low-pressure ultraviolet light

    CN113233563A

Cited By

  • Preparation method of bionic flocculant for benzene ring medicine wastewater treatment

    CN119285057A

  • Shape memory water-based hydraulic damping fluid containing electromagnetic rheological polymer composite particles and preparation method of shape memory water-based hydraulic damping fluid

    CN119639216A

  • Polyaluminum chloride composite flocculant for phosphorus-containing wastewater treatment and preparation method thereof

    CN121044692A