Regeneration method of vanadium electrolyte waste liquid

Through filtration and electrolytic treatment, combined with the use of flocculants, the problem of removing high-content impurities in the waste liquid of vanadium electrolyte is successfully solved, and the regeneration of high-purity electrolyte is realized, which simplifies the process, reduces costs, and avoids electron beam radiation. The dangers of the photo.

CN118908447AActive Publication Date: 2024-11-08DALI ENERGY STORAGE TECH HUBEI CO LTD

Patent Information

Application Number
CN202411001006.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The prior art cannot effectively deal with vanadium electrolyte waste liquid with high impurities, resulting in complex and costly electrolyte regeneration process, and electron beam radiation problems that are harmful to the human body.

Method used

The first filtration is used to remove insoluble impurities, and the vanadium ion valence state is adjusted to below 3 valence by electrolytic reduction. The flocculant is added for flocculation reaction and the second filtration is performed. The copper ions are then removed by electrolysis, and the vanadium ion valence state is adjusted to below 3.5 valence. , a high-purity vanadium electrolyte solution was obtained.

Benefits of technology

It realizes the regeneration of high-purity vanadium electrolyte, which is simple to operate, low energy consumption, pollution-free, and has high efficiency. It is suitable for large-scale use, reducing the operating cost of vanadium battery system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908447A_ABST
    Figure CN118908447A_ABST
Patent Text Reader

Abstract

The invention provides a regeneration method of a vanadium electrolyte waste liquid, which comprises the following steps: by taking a vanadium battery waste liquid as a raw material, filtering out insoluble impurities in the waste liquid through primary filtration, and adjusting the valence state of an electrolyte to be lower than trivalence through primary electrolysis, thereby avoiding flocculation caused by high valence state of vanadium ions; adding a flocculating agent, stirring to generate a flocculation reaction, flocculating impurity ions, filtering for the second time, electrolyzing the filtered vanadium electrolyte for the second time through an electrolyzing device, separating out copper ions on a cathode electrode, washing by the electrolyte, bringing separated copper into a cathode liquid storage tank, and settling; and thus, copper ions introduced into the flocculating agent are removed, the electrolyte is adjusted to the target valence state, and finally the regenerated high-purity vanadium electrolyte is obtained. The whole method is simple to operate, low in energy consumption, free of pollution, high in efficiency and short in regeneration time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste electrolyte regeneration, in particular to a method for regenerating waste vanadium electrolyte. Background Art

[0002] All-vanadium redox flow batteries have the advantages of high energy conversion efficiency, adjustable capacity, long service life, high safety and environmental friendliness. They are mainly used in energy storage equipment for power generation systems of renewable energy such as solar energy and wind energy, peak-shaving and valley-filling devices for power grids, and uninterruptible power supplies and emergency power supply systems.

[0003] In vanadium batteries, energy is stored in vanadium electrolyte. The electrolyte is the main component of all-vanadium flow batteries. It is composed of vanadium ions and sulfuric acid or hydrochloric acid. The positive electrode is VO 2+ / VO2 + The redox couple is composed of a negative electrode of V 3+ / V 2+ The redox couple is composed of redox pairs. The battery is the place where the electrolyte is charged and discharged. The electrolyte is transported by pumps and pipes and circulates between the storage tank and the battery. The initial valence of the vanadium ion in the electrolyte is trivalent: tetravalent, which is a 1:1 electrolyte, that is, a 3.5-valent electrolyte.

[0004] However, with the long-term use of vanadium battery systems, storage tanks, pipelines, pumps, battery stack materials, etc. will continue to age, and the impurity ions therein will continue to enter the vanadium electrolyte, rendering the vanadium electrolyte unusable and forming waste liquid. Furthermore, during the operation of the vanadium battery system, pipeline damage, battery stack leakage, etc. may occur, causing a large amount of electrolyte leakage. The leaked electrolyte comes into contact with the ground, introducing a large amount of impurities, making it impossible to continue to use, thereby forming a large amount of waste liquid.

[0005] At present, there are two main ways to treat vanadium electrolyte waste:

[0006] One is to perform a series of vanadium precipitation operations on the spent electrolyte, and finally obtain vanadium compounds such as vanadium pentoxide, vanadyl sulfate, and ammonium metavanadate. However, although the above method can obtain vanadium compounds, the purity of the obtained product is not high, and the product cannot be directly used as a raw material for vanadium electrolyte. It needs to be further purified and impurity-removed before it can be used as a raw material for vanadium battery electrolyte. In addition, the production of electrolyte using vanadium compounds as raw materials requires additional electrolyte production processes, and the environmental protection cost and manufacturing cost are relatively high.

[0007] Second, after the spent electrolyte is regenerated, it is continued to be used in the vanadium battery system, thereby achieving the purpose of extending the service life of the electrolyte, reducing the cost of vanadium precipitation and the cost of electrolyte manufacturing, and is a better choice for the disposal of vanadium waste liquid. Chinese patent document CN116914171A discloses a method for the regeneration of spent electrolytes. The patent preliminarily treats the spent electrolyte by pickling, ion exchange, membrane filtration, etc., and then uses electron beam irradiation to eliminate organic impurities, and finally uses an adsorbent to filter and purify, so as to eliminate impurities in the spent electrolyte and achieve the purpose of electrolyte regeneration. This method has complicated steps, produces a lot of wastewater, and electron beam irradiation is harmful to the human body to a certain extent, so this method is not conducive to large-scale use. Chinese patent document CN102468499A discloses a method for regenerating waste liquid of an all-vanadium flow battery. The patent reduces the 5-valent vanadium ions in the electrolyte to 4-valent by contacting the positive electrode electrolyte of the all-vanadium flow battery after the first charge with a reducing agent such as oxalic acid, formic acid, and tartaric acid. The obtained 4-valent vanadium ion electrolyte is used as the positive or negative electrolyte of the vanadium battery. However, this method does not take into account the influence of impurities. The 4-valent vanadium ion electrolyte obtained by reducing the waste liquid with high impurity content cannot be used directly as the electrolyte of the vanadium battery, otherwise it will greatly affect the performance and service life of the vanadium battery. Chinese patent document CN111509247A discloses a method for regenerating the electrolyte of a failed vanadium battery. The positive and negative electrolytes of the failed vanadium battery are mixed, and a vanadium compound, a supporting electrolyte and water are added. After solid-liquid separation, the liquid phase is subjected to capacitor deionization and electrolytic reduction in the electrolytic cell in turn, and finally a 3.5-valent vanadium electrolyte is obtained. However, the manufacturing process of the anode composite electrode and the cathode composite electrode involved in this method is complicated, especially for waste liquid with high impurity content, the composite electrode consumption is large and the regeneration cost of the failed electrolyte is high.

[0008] Therefore, it is necessary to design a regeneration method for vanadium electrolyte waste liquid, which can effectively treat high-content impurities and achieve the regeneration of failed electrolyte so that it can continue to be used in the vanadium battery system, thereby solving the defects of the existing technical methods such as complexity and high cost. Summary of the invention

[0009] The present invention provides a method for regenerating waste vanadium electrolyte, which solves the problem that the prior art cannot effectively process high-content impurities, and enables the failed electrolyte to continue to be used in the vanadium battery system after being regenerated, thereby solving the defects of the prior art method being complex and costly.

[0010] The technical solution of the present invention is achieved in this way:

[0011] The first aspect of the present invention provides a method for regenerating vanadium electrolyte waste liquid, comprising the steps of:

[0012] S1. Filter the waste liquid for the first time to remove insoluble impurities;

[0013] S2. The filtered waste liquid is subjected to a first electrolytic reduction until the valence of the vanadium ion drops below 3;

[0014] S3. Add an excess of flocculant to the waste liquid obtained in step S2 under stirring, and after sufficient reaction, perform a second filtration to remove the flocculation product; the flocculant includes a copper flocculant and an amide polymer flocculant;

[0015] S4. The mother liquor after filtering in step S3 is subjected to a second electrolytic reduction to deposit and remove copper;

[0016] S5. Adjusting the valence state of vanadium ions in the electrolyte treated in step S4 to obtain a regenerated vanadium electrolyte.

[0017] Furthermore, the first electrolytic reduction process is to place the waste liquid at the cathode of the electrolytic cell for electrolysis, and the anode is an aqueous solution with the same acid concentration. By placing the waste liquid at the cathode of the electrolytic cell to cause a reduction reaction, the valence state of the vanadium ion is adjusted to 3 or less.

[0018] Furthermore, the second electrolytic reduction process is to place the mother liquor in a cathode liquid storage tank, circulate the mother liquor between the cathode liquid storage tank and the cathode chamber of the electrolytic cell, and set a solution with the same acid concentration as the mother liquor to circulate between the anode liquid storage tank and the anode chamber of the electrolytic cell.

[0019] Furthermore, the vanadium ion valence adjustment process is to place the electrolyte at the anode of the electrolytic cell for electrolysis, and the cathode is an aqueous solution with the same acid concentration.

[0020] Furthermore, the copper flocculant includes at least one of copper sulfate and copper hydroxide; the amide polymer flocculant includes at least one of polyacrylamide and polyvinylamide; the amide polymer flocculant is preferably cationic polyacrylamide.

[0021] Furthermore, the amide polymer flocculant is cationic polyacrylamide, and when copper sulfate is selected as the copper flocculant, the mass ratio of copper sulfate to cationic polyacrylamide is greater than 2.5:1; when copper hydroxide is selected as the copper flocculant, the mass ratio of copper hydroxide to cationic polyacrylamide is greater than 1.5:1.

[0022] Furthermore, the first filtration is used to remove insoluble impurities, using at least one of a mesh filter, a laminated filter, a sand rod filter, a carbon filter, a plate and frame filter, and an activated carbon filter; and / or, the second filtration is used to remove condensed colloidal floccules containing a large amount of impurity ions, using at least one of a mesh filter, a laminated filter, a sand rod filter, a carbon filter, a plate and frame filter, and an activated carbon filter.

[0023] Furthermore, the vanadium concentration in the vanadium electrolyte waste liquid is 1-4.0 mol / L, and the vanadium includes the sum of vanadium ions of any valence state. The vanadium electrolyte waste liquid includes one or more impurities of calcium ions, silicon ions, iron ions, aluminum ions and chromium ions; the silicon ions exist in the form of one or more of water-soluble silicon, amorphous silicon and colloidal silicon.

[0024] The second object of the present invention is to propose the application of the regeneration method described in the first aspect in the preparation of vanadium electrolyte.

[0025] Furthermore, the valence state of vanadium ions in the vanadium electrolyte is 3.5, which satisfies the initial valence state of vanadium ions in the electrolyte.

[0026] Compared with the prior art, the beneficial effects of the present invention include at least:

[0027] The method for regenerating vanadium electrolyte waste liquid of the present invention uses vanadium battery waste liquid as raw material, performs a first filtration to filter out insoluble impurities in the waste liquid, adjusts the electrolyte valence to less than trivalence through a first electrolysis to avoid flocculation due to high valence of vanadium ions; adds a flocculant to stir and generate a flocculation reaction, performs a second filtration after flocculating the impurity ions, and performs a second electrolysis of the filtered vanadium electrolyte through an electrolysis device, wherein copper ions are precipitated on a cathode electrode, and the precipitated copper is brought into a cathode liquid storage tank and precipitated by flushing with the electrolyte, thereby removing the copper ions introduced in the flocculant, and the electrolyte is adjusted to a target valence to finally obtain a regenerated high-purity vanadium electrolyte; the whole method is simple to operate, has low energy consumption, is pollution-free, has high efficiency, and has a short regeneration time. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 The present invention provides an overall flow chart of the method for regenerating waste vanadium electrolyte. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Reference Figure 1In one embodiment, a method for regenerating vanadium electrolyte waste is proposed, the steps comprising:

[0032] S1. Filter the waste liquid for the first time to remove insoluble impurities;

[0033] S2. The filtered waste liquid is subjected to a first electrolytic reduction until the valence of the vanadium ion drops below 3;

[0034] S3. Add an excess of flocculant to the waste liquid obtained in step S2 under stirring, and after sufficient reaction, perform a second filtration to remove the flocculation product; the flocculant includes a copper flocculant and an amide polymer flocculant;

[0035] S4. The mother liquor after filtering in step S3 is subjected to a second electrolytic reduction to deposit and remove copper;

[0036] S5. Adjusting the valence state of vanadium ions in the electrolyte treated in step S4 to obtain a regenerated vanadium electrolyte.

[0037] In the above embodiment, the regeneration method is to filter out insoluble impurities in the waste liquid through the first filtration, adjust the electrolyte valence to less than trivalent through the first electrolysis, and avoid flocculation due to the high valence of vanadium ions; add a flocculant to stir and produce a flocculation reaction, flocculate the impurity ions and then perform a second filtration, the filtered vanadium electrolyte is passed through an electrolysis device for secondary electrolysis, copper ions are precipitated on the cathode electrode, and the precipitated copper is brought into the cathode liquid storage tank and precipitated by flushing with the electrolyte, thereby removing the copper ions introduced in the flocculant, and the electrolyte is then adjusted to the target valence, and finally a regenerated high-purity vanadium electrolyte is obtained; the whole method is simple to operate, low in energy consumption, pollution-free, efficient, and short in regeneration time.

[0038] In a preferred embodiment, the copper flocculant can be selected from at least one of copper sulfate and copper hydroxide; the amide polymer flocculant includes at least one of polyacrylamide and polyvinylamide, preferably cationic polyacrylamide. By using a mixture of copper hydroxide or copper sulfate and polyacrylamide, polyvinylamide and other amide polymers as a flocculant, common impurity ions such as iron, calcium, silicon, aluminum, and chromium in the trivalent vanadium electrolyte waste liquid are removed. The excess copper ions in the filtrate are electrolyzed and precipitated on the cathode electrode of the electrolytic cell by electrodeposition reaction, and the precipitated elemental copper is flushed into the cathode reservoir tank by the flow of the electrolyte between the cathode reservoir tank and the cathode chamber. Since the density of elemental copper is much greater than that of the electrolyte, elemental copper is deposited at the bottom of the cathode reservoir tank, thereby achieving the purpose of removing copper ions in the electrolyte, and then achieving the purpose of regenerating the vanadium electrolyte waste liquid. The flocculant used is simple and easy to obtain, cheap, and easy to operate. Through flocculation reaction and electrodeposition, the impurity ions in the waste liquid can be effectively removed.

[0039] In the above embodiment, the valence state adjustment, flocculation precipitation and copper deposition are mainly carried out by considering the synergy of the following effects: the copper ions in the flocculant copper hydroxide or copper sulfate can form a macromolecular complex with PAM under acidic conditions, and the complex can undergo flocculation and chelation with various ions such as calcium ions, silicon ions, iron ions, aluminum ions, chromium ions, etc., thereby generating a colloidal precipitate, while the complex will not undergo chelation with divalent and trivalent vanadium ions, but will only undergo flocculation and chelation with tetravalent and pentavalent vanadium ions; thus, the valence state of the vanadium electrolyte waste liquid can be adjusted to trivalent or below, and then the macromolecular complex generated by the copper ions in the copper hydroxide or copper sulfate and PAM is flocculated to remove impurity ions other than copper ions, and the excess copper ions are removed by electrolytic deposition, thereby achieving the effect of removing impurity ions in the trivalent vanadium electrolyte.

[0040] In a preferred embodiment, in order to ensure that the added amide polymer flocculant can be completely removed with the subsequent flocculation and chelation products, when added, the copper flocculant is excessive relative to the amide polymer flocculant, that is, an excess of copper flocculant is first added to allow the amide polymer flocculant to fully flocculate to form a macromolecular complex. Specifically, if cationic polyacrylamide (CPAM) is selected, when copper sulfate is selected as the copper flocculant, the mass ratio of copper sulfate to CPAM is greater than 2.5:1; when copper hydroxide is selected as the copper flocculant, the mass ratio of copper hydroxide to CPAM is greater than 1.5:1.

[0041] In a preferred embodiment, the amount of the flocculant is preferably excessive, that is, the flocculant is continuously added during the stirring and flocculation process until the content of free metal impurity ions in the electrolyte waste liquid no longer decreases. This process can be achieved with the help of detection means. Considering the content of metal impurity ions in general waste liquid, the amount of flocculant added can be considered to be 0.1-1% of the mass of the waste liquid. If the electrolyte introduced with impurities is used for a long time, the impurity content is small, and the amount of flocculant added is 0.1-0.5%; if the impurities introduced from the ground are large, the amount of flocculant added is 0.5-1%.

[0042] In a preferred embodiment, the electrolysis process generates an oxidation reaction at the anode and a reduction reaction at the cathode. Personnel in the art can select the appropriate units and reagents required for electrolysis according to the reaction principle and the desired reduction / oxidation effect. As is well known in the art, the electrolysis device includes an electrolytic cell, an anode liquid storage tank, a cathode liquid storage tank, an anode circulation pump, a cathode circulation pump, and a DC power supply. The electrolytic cell includes an anode plate, an anode electrode, a cathode plate, a cathode electrode, an anode chamber, a cathode chamber, and a diaphragm; the anode plate of the electrolytic cell is one of a lead plate, a titanium plate, a stainless steel or a graphite plate; the anode electrode of the electrolytic cell is one of a titanium felt, a nickel felt, a graphite felt, and a stainless steel fiber felt; the cathode plate of the electrolytic cell is one of a lead plate, a DSA, and a graphite plate; the anode electrode of the electrolytic cell is one of a titanium felt, a nickel felt, a graphite felt, and a stainless steel fiber felt; the electrolytic cell diaphragm is one of a cation exchange membrane, a proton exchange membrane, an anion exchange membrane, and a PBI membrane.

[0043] In the above embodiments, the vanadium electrolyte waste liquid may come from the waste liquid formed by the continuous aging of storage tanks, pipelines, pumps, battery stack materials, etc., and the introduction of impurity ions that make the vanadium electrolyte unusable; it may also come from the damage of pipelines and leakage of battery stacks during the operation of the vanadium battery system, resulting in a large amount of electrolyte leakage, and the introduction of a large amount of impurities in contact with the ground to form a large amount of waste liquid. The waste liquid includes but is not limited to one or more impurities of calcium ions, silicon ions, iron ions, aluminum ions and chromium ions; the silicon ions exist in the form of one or more of water-soluble silicon, amorphous silicon, and colloidal silicon. The sum of the concentrations of vanadium ions of any valence state in the vanadium electrolyte waste liquid is not limited to a certain concentration. In actual vanadium battery electrolytes, the vanadium concentration is usually 1 to 4.0 mol / L; impurity ions include the above-mentioned combination of impurity ions. The electrolyte waste liquid regeneration is applicable, and the impurity ion concentration is significantly reduced after regeneration.

[0044] The following is a preferred implementation example of the present invention. The electrolyte waste liquid is vanadium electrolyte waste liquid leaked to the ground. 3 The total molar number of vanadium in the electrolyte waste solution was initially measured to be 2.0×10 3 mol.

[0045] Unless otherwise specified, all reagents used are commercially available standards, and the experimental procedures involved are basic operations that are well known and mastered by those skilled in the art.

[0046] Example 1

[0047] The regeneration process is as follows: use a 1000 mesh screen filter for the first filtration to filter out insoluble impurities, place the waste liquid at the cathode of the electrolytic cell for electrolysis, electrolyze the vanadium ions to trivalence, add 3.0 kg of copper hydroxide and 2.0 kg of cationic polyacrylamide mixed powder, stir for 30 minutes, fully flocculate, use a 3000 mesh screen filter for the second filtration, the filtered vanadium liquid is placed in the cathode liquid storage tank of the electrolysis device, and the vanadium liquid is circulated between the cathode liquid storage tank and the cathode chamber of the electrolytic cell through the cathode circulation pump, and the sulfuric acid aqueous solution with the same sulfate radical is circulated between the anode liquid storage tank and the anode chamber of the electrolytic cell through the anode circulation pump. The anode plate of the electrolytic cell is a lead plate, the anode electrode of the electrolytic cell is a titanium felt, the cathode plate of the electrolytic cell is a graphite plate, the cathode electrode of the electrolytic cell is a graphite felt, the cathode and anode of the electrolytic cell are connected to the negative pole and the positive pole of the DC power supply respectively, and the electrolytic cell is electrolyzed by passing 100A DC. After 30 minutes, the electrolysis was stopped, and the single copper obtained by electrodeposition was collected at the bottom of the cathode liquid storage tank. The electrolyte was taken for impurity ion detection. The electrolyte was placed at the anode of the electrolytic cell for electrolysis, and the valence state of the vanadium ion was adjusted to 3.5, and the total vanadium recovery rate was measured to be greater than 99.99%.

[0048] Example 2

[0049] The regeneration process is as follows: use a 1000 mesh screen filter for the first filtration to filter out insoluble impurities, place the waste liquid at the cathode of the electrolytic cell for electrolysis, electrolyze the vanadium ions to trivalence, add 3.6 kg of copper sulfate and 1.4 kg of cationic polyacrylamide mixed powder, stir for 30 minutes, fully flocculate, use a 3000 mesh screen filter for the second filtration, the filtered vanadium liquid is placed in the cathode liquid storage tank of the electrolysis device, and the vanadium liquid is circulated between the cathode liquid storage tank and the cathode chamber of the electrolytic cell through the cathode circulation pump, and the sulfuric acid aqueous solution with the same sulfate radical is circulated between the anode liquid storage tank and the anode chamber of the electrolytic cell through the anode circulation pump. The anode plate of the electrolytic cell is a lead plate, the anode electrode of the electrolytic cell is a titanium felt, the cathode plate of the electrolytic cell is a graphite plate, the cathode electrode of the electrolytic cell is a graphite felt, the cathode and anode of the electrolytic cell are connected to the negative pole and the positive pole of the DC power supply respectively, and the electrolytic cell is electrolyzed by 100A DC. After 30 minutes, the electrolysis was stopped, and the single copper obtained by electrodeposition was collected at the bottom of the cathode liquid storage tank. The electrolyte was taken for impurity ion detection. The electrolyte was placed at the anode of the electrolytic cell for electrolysis, and the valence state of the vanadium ion was adjusted to 3.5, and the total vanadium recovery rate was measured to be greater than 99.99%.

[0050] Example 3

[0051] The regeneration process is as follows: a 1000-mesh screen filter is used for the first filtration to remove insoluble impurities, and the waste liquid is placed at the cathode of the electrolytic cell for electrolysis. The vanadium ions are electrolyzed to trivalence, and a powder of 1.5 kg copper hydroxide, 2.0 kg copper sulfate and 1.5 kg cationic polyacrylamide is added, stirred for 30 minutes, and fully flocculated. A 3000-mesh screen filter is used for the second filtration, and the filtered vanadium liquid is placed in the cathode liquid storage tank of the electrolysis device. The vanadium liquid is circulated between the cathode liquid storage tank and the cathode chamber of the electrolytic cell through the cathode circulation pump, and the sulfuric acid aqueous solution with the same sulfate radical is circulated between the anode liquid storage tank and the anode chamber of the electrolytic cell through the anode circulation pump. The anode plate of the electrolytic cell is a lead plate, the anode electrode of the electrolytic cell is a titanium felt, the cathode plate of the electrolytic cell is a graphite plate, and the cathode electrode of the electrolytic cell is a graphite felt. The cathode and anode of the electrolytic cell are connected to the negative pole and the positive pole of the DC power supply respectively, and the electrolytic cell is electrolyzed by passing 100A DC. After 30 minutes, the electrolysis was stopped, and the single copper obtained by electrodeposition was collected at the bottom of the cathode liquid storage tank. The electrolyte was taken for impurity ion detection. The electrolyte was placed at the anode of the electrolytic cell for electrolysis, and the valence state of the vanadium ion was adjusted to 3.5, and the total vanadium recovery rate was measured to be greater than 99.99%.

[0052] Comparative Example 1

[0053] The steps and methods used in this embodiment are basically the same as those in Embodiment 1, except that copper hydroxide is not added to the flocculant.

[0054] Comparative Example 2

[0055] The steps and methods used in this embodiment are basically the same as those in Embodiment 1, except that no polyacrylamide is added to the flocculant.

[0056] Comparative Example 3

[0057] The steps and methods used in this embodiment are basically the same as those in Embodiment 1, except that the valence state of the vanadium ions is not adjusted before adding the flocculant.

[0058] In the above embodiments and comparative examples 1 to 3, the comparison results of impurity ions in the vanadium electrolyte waste liquid before treatment and the electrolyte after treatment are shown in Table 1. It can be seen from the comparison of ICP data shown in Table 1 that the method can effectively remove impurity ions in the vanadium waste liquid, the treated electrolyte meets the continued use of vanadium batteries, and the vanadium recovery rate in the electrolyte regeneration process is high.

[0059] Table 1: Comparison of impurity ions before and after treatment of vanadium electrolyte wastewater in Example

[0060]

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for regenerating vanadium electrolyte waste liquid, characterized in that the steps include: S1. Filter the waste liquid for the first time to remove insoluble impurities; S2. The filtered waste liquid is subjected to a first electrolytic reduction until the valence of the vanadium ion drops below 3; S3. Add an excess of flocculant to the waste liquid obtained in step S2 under stirring, and after sufficient reaction, perform a second filtration to remove the flocculation product; the flocculant includes a copper flocculant and an amide polymer flocculant; S4. The mother liquor after filtering in step S3 is subjected to a second electrolytic reduction to deposit and remove copper; S5. Adjusting the valence state of vanadium ions in the electrolyte treated in step S4 to obtain a regenerated vanadium electrolyte.

2. The regeneration method according to claim 1, characterized in that: The first electrolytic reduction process is to place the waste liquid at the cathode of the electrolytic cell for electrolysis, and the anode is an aqueous solution with the same acid concentration.

3. The regeneration method according to claim 1, characterized in that: The second electrolytic reduction process is to place the mother liquor in the cathode liquid storage tank, circulate the mother liquor between the cathode liquid storage tank and the cathode chamber of the electrolytic cell, and set a solution with the same acid concentration as the mother liquor to circulate between the anode liquid storage tank and the anode chamber of the electrolytic cell.

4. The regeneration method according to claim 1, characterized in that: The vanadium ion valence adjustment process is to place the electrolyte at the anode of the electrolytic cell for electrolysis, and the cathode is an aqueous solution with the same acid concentration.

5. The regeneration method according to claim 1, characterized in that: The copper flocculant includes at least one of copper sulfate and copper hydroxide; the amide polymer flocculant includes at least one of polyacrylamide and polyvinylamide.

6. The regeneration method according to claim 5, characterized in that: The amide polymer flocculant is cationic polyacrylamide. When copper sulfate is selected as the copper flocculant, the mass ratio of copper sulfate to cationic polyacrylamide is greater than 2.5:1; when copper hydroxide is selected as the copper flocculant, the mass ratio of copper hydroxide to cationic polyacrylamide is greater than 1.5:

1.

7. The regeneration method according to claim 1, characterized in that: The vanadium concentration in the vanadium electrolyte waste liquid is 1-4.0 mol / L.

8. The regeneration method according to claim 1, characterized in that: The vanadium electrolyte waste liquid includes one or more impurities selected from the group consisting of calcium ions, silicon ions, iron ions, aluminum ions and chromium ions.

9. Use of the regeneration method according to any one of claims 1 to 8 in the preparation of vanadium electrolyte.

10. The use according to claim 9, characterized in that The valence state of vanadium ions in the vanadium electrolyte is 3.5.

Citation Information

Patent Citations

  • Combined chemical-electrochemical method for preparing vanadium redox flow battery electrolyte

    CN104037439A

  • Method of removing copper ions in vanadium electrolyte

    CN107768702A

  • Treatment method for extracting lead acid from waste acid of waste lead-acid battery

    CN115353143A

  • Method and device for preparing vanadium electrolyte from crude vanadium

    CN117902626A

Cited By

  • Electrolyte purification device and purification method thereof

    CN119230880A

  • A kind of electrolyte purification device and purification method

    CN119230880B

  • Multi-parameter online detection system and method for all-vanadium redox flow battery electrolyte

    CN121027409A