Cement composite material for decoration, preparation method and building decoration structure

By using decorative cement composite materials composed of white silicate cement and titanium dioxide, the problems of difficult color adjustment of decorative materials and rusting of steel fibers in existing technologies have been solved, realizing an integrated decorative structure with high strength and low maintenance cost.

CN118908651APending Publication Date: 2024-11-08CHANGSHA ENDONG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958791.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing high-performance nanocomposite materials have problems in building exterior decoration, such as difficulty in adjusting the basic color tone, poor gloss after construction, and rusting and falling off of steel fibers, resulting in complex construction, high cost and great safety hazards.

Method used

Decorative cement composite materials, composed of white silicate cement, titanium dioxide, defoamer, etc., are used to form an integrated decorative structure through mixing, molding and steam curing processes, thus avoiding the use of steel fibers.

Benefits of technology

This method achieves a base color close to white, facilitating color matching, resulting in a high surface finish, preventing steel fibers from rusting, reducing the number of construction operations, lowering maintenance costs, and improving structural strength and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908651A_ABST
    Figure CN118908651A_ABST
Patent Text Reader

Abstract

The invention provides a cement composite material for decoration, a preparation method and a building decoration structure. The cement composite material for decoration comprises the following preparation raw materials in parts by mass: 1.0 part of white Portland cement; 0.1 to 0.5 part of white silica fume; 0.2 to 0.5 part of 325-mesh quartz powder; 0.6 to 1.5 parts of quartz sand; 0.05 to 0.18 part of kaolin; 0.02 to 0.08 part of nano CaO (calcium oxide); 0.01 to 0.04 part of nano Na2O (sodium oxide); 0.02 to 0.06 part of calcium carbonate; 0.005 to 0.08 part of a defoaming agent; 0.01 to 0.045 part of a water reducing agent; 0.02 to 0.1 part of synthetic fiber; 0.003 to 0.12 part of titanium dioxide; and 0.16 to 0.22 part of water. The performance of an existing active nano inorganic composite material is improved, so that the active nano inorganic composite material can be applied to a decorative structure, and the defects of the existing decorative structure are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of building and decoration materials, and in particular to a decorative cement composite material, a preparation method and a building decoration structure. Background Art

[0002] The conventional practice of building decoration construction is to first construct the main structure of the decoration, and then construct the outer layer of decorative materials on top of the main structure. In this way, two constructions are required, resulting in a large waste of materials and high maintenance costs. In addition, in many cases, the strength of the main structure of the decoration and the outer layer of decorative materials is low, and the construction quality is difficult to control. In addition, the outer layer of decorative materials will age and fall off prematurely compared to the main structure, with a short lifespan and prone to safety problems.

[0003] Active nano inorganic composite material is an inorganic composite material with silicate cement as the main binder, high-strength orthopedics, active nano materials (powders and fibers) and metal fibers for reinforcement and toughening, and cured by high temperature or high temperature and high pressure saturated steam. It belongs to ultra-high performance cement-based composite materials. At present, high-performance nano composite materials have been released at home and abroad, and developed after ultra-fine solid volume materials. However, there are many problems with existing high-performance nano composite materials, which are not suitable for application in the exterior decoration of buildings. Specifically, Chinese patent 201410791309.7 discloses a cement-based nano composite material. The material disclosed in the patent document will have the following problems when used for decoration: First, the base color of the cement-based nano composite material is not white, which is very difficult to adjust the color in the later stage. Second, there will be a large number of bubbles after the cement-based nano composite material is formed, and the finish is not high after construction. Third, the cement-based nano composite material contains steel fibers, which have rust problems and poor durability. When the steel fibers fall off, they are easy to cause injuries. Summary of the invention

[0004] The technical problem to be solved by the present application is to propose a decorative cement composite material, a preparation method and a building decoration structure in view of the above-mentioned deficiencies in the prior art.

[0005] A decorative cement composite material, the decorative cement composite material comprises the following raw materials and their corresponding weight parts:

[0006] White Portland cement: 1.0;

[0007] White silica fume: 0.1 - 0.5;

[0008] 325 mesh quartz powder: 0.2 - 0.5;

[0009] Quartz sand: 0.6-1.5;

[0010] Kaolin: 0.05-0.18;

[0011] Nano-CaO: 0.02-0.08;

[0012] Nano Na2O: 0.01-0.04;

[0013] Calcium carbonate: 0.02-0.06;

[0014] Defoamer: 0.005-0.08;

[0015] Water reducing agent: 0.01–0.045;

[0016] Synthetic fiber: 0.02 -0.1;

[0017] Titanium dioxide: 0.003-0.12;

[0018] Water: 0.16-0.22.

[0019] Optionally, the decorative cement composite material further comprises a pigment.

[0020] Optionally, the water reducer is a polyanal acid special water reducer with a solid content of 45% and a water reduction rate of ≥35%.

[0021] Optionally, the particle size of the quartz sand ranges from 0.4 mm to 0.6 mm.

[0022] Optionally, the mass fraction of the white silica fume is: 0.1, 0.2, 0.3, 0.4, 0.5;

[0023] The mass fractions of the 325 mesh quartz powder are specifically: 0.2, 0.3, 0.4, 0.5;

[0024] The mass fractions of the quartz sand are specifically: 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5;

[0025] The mass fractions of the kaolin are specifically: 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18;

[0026] The specific mass fractions of the nano-CaO are: 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08;

[0027] The specific mass fractions of the nano-Na2O are: 0.01, 0.02, 0.03, 0.04;

[0028] The specific mass fractions of calcium carbonate are: 0.02, 0.03, 0.04, 0.05, 0.06;

[0029] The mass parts of the defoaming agent are specifically: 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08;

[0030] The mass fractions of the water reducing agent are specifically: 0.01, 0.02, 0.03, 0.04, 0.045;

[0031] The mass fractions of the synthetic fibers are specifically: 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10;

[0032] The specific mass fractions of the titanium dioxide are: 0.003, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12;

[0033] The specific mass parts of water are: 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, and 0.22.

[0034] On the other hand, the present application also provides a preparation method, which is applied to the above-mentioned decorative cement composite material, comprising:

[0035] The raw materials are stirred and mixed according to the mass ratio, and the mixture is poured into a mold for molding. After hardening, it is demoulded and cured.

[0036] Optionally, pigment is added and stirred during the stirring and mixing process of the raw materials.

[0037] Optionally, the preparation method specifically comprises the steps of:

[0038] Step 101a, white silicate cement, white silica fume, nano-CaO, calcium carbonate, kaolin, and defoamer are mixed and stirred in sequence according to the mass ratio;

[0039] Step 102a, adding 325 mesh quartz powder to the uniformly stirred powder according to the mass ratio, and then adding quartz sand, nano-Na2O, and titanium dioxide and stirring evenly;

[0040] Step 104a, adding water reducing agent and water according to the mass ratio, and stirring evenly until the mixture is fluidized;

[0041] Step 105a, after the materialization, continue to stir while uniformly adding the synthetic fibers to stir and disperse them uniformly;

[0042] Step 106a, pouring the uniformly stirred mixture into a mold, removing bubbles and forming by vibrating and vacuuming, and demoulding after hardening;

[0043] Step 107a, steam curing the hardened product at 60°C-80°C for 2-4 days.

[0044] Optionally, the preparation method specifically comprises the steps of:

[0045] Step 101b, mixing white silicate cement, white silica fume, nano-CaO, calcium carbonate, kaolin, and defoamer in sequence according to the mass ratio and stirring evenly;

[0046] Step 102b, adding 325 mesh quartz powder to the uniformly stirred powder according to the mass ratio, and then adding quartz sand, nano-Na2O, and titanium dioxide and stirring evenly;

[0047] Step 103b, adding the prepared color pigment in portions and stirring evenly;

[0048] Step 104b, adding water reducing agent and water according to the mass ratio, and stirring evenly until the mixture is fluidized;

[0049] Step 105b, after the materialization, continue to stir while uniformly adding the synthetic fibers to stir and disperse them uniformly;

[0050] Step 106b, pouring the uniformly stirred mixture into a mold, removing bubbles and forming by vibrating and vacuuming, and demoulding after hardening;

[0051] Step 107b, steam curing the hardened product at 60°C-80°C for 2-4 days.

[0052] On the other hand, the present application also provides a building decoration structure, which is made using the above-mentioned preparation method.

[0053] This application improves the performance of existing active nano inorganic composite materials, so that they can be applied to decorative structures and improve the shortcomings of existing decorative structures. Compared with existing active nano inorganic composite materials, the decorative cement composite material provided by this application has the following advantages:

[0054] First, the decorative cement composite material provided by the present application adopts white silicate cement, and the addition of titanium dioxide can achieve a whitening effect, so that the basic color of the cement-based nanocomposite material is close to white, which is convenient for obtaining various color effects.

[0055] Second, it does not contain steel fibers, does not rust, and has better durability.

[0056] Third, the use of defoaming agent reduces bubbles, and the surface finish is high after construction.

[0057] When the decorative cement composite material provided by the present application is used for decoration, an integrated structure can be realized. Only one construction is required to form an integrated decorative structure, which replaces the main structure and outer layer decoration of the existing decoration, overcomes the problem of premature aging of the outer layer decorative material in the existing decorative structure, does not have the problem of the existing outer layer decoration falling off, eliminates safety hazards, and achieves lower costs, less space occupation, less weight, and higher strength. In addition, when the decorative cement composite material of the present application is used for decoration, its decorative structure is maintenance-free, and surface defects can be eliminated by removing a layer of surface material. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 It is one of the flow charts of the preparation method in the examples of the present application.

[0059] Figure 2 This is the second flow chart of the preparation method in the examples of the present application. DETAILED DESCRIPTION

[0060] The following is the specific embodiment of the present application and in conjunction with the accompanying drawings, the technical scheme of the present application is further described, but the present application is not limited to these embodiments. In the following description, specific details such as specific configuration and assembly are provided only to help fully understand the embodiments of the present application. Therefore, it should be clear to those skilled in the art that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the present application. In addition, for clarity and brevity, the description of known functions and structures has been omitted.

[0061] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments in this application can be combined with each other.

[0062] In the prior art, the conventional practice of building decoration construction is: first construct the main structure of the decoration, and then construct the outer layer of decorative materials on the main structure. In this way, two constructions are required, which results in large waste of materials and high maintenance costs. In addition, in many cases, the strength of the main structure of the decoration and the outer layer of decorative materials is low, and the construction quality is difficult to control. The present application improves the existing active nano inorganic composite material so that it can be applied to decorative structures and improves the shortcomings of the existing decorative structures. The following is a detailed description with reference to the accompanying drawings.

[0063] The decorative cement composite material provided in this application includes the following raw materials and their corresponding weight parts:

[0064] White Portland cement: 1.0;

[0065] White silica fume: 0.1-0.5;

[0066] 325 mesh quartz powder: 0.2-0.5;

[0067] Quartz sand: 0.6-1.5;

[0068] Kaolin: 0.05-0.18;

[0069] Nano-CaO: 0.02-0.08;

[0070] Nano Na2O: 0.01-0.04;

[0071] Calcium carbonate: 0.02-0.06;

[0072] Defoamer: 0.005-0.08;

[0073] Water reducing agent: 0.01–0.045;

[0074] Synthetic fiber: 0.02 -0.1;

[0075] Titanium dioxide: 0.003-0.12;

[0076] Water: 0.16-0.22.

[0077] In one embodiment of the present application, the decorative cement composite material further includes a pigment.

[0078] In one embodiment of the present application, the water reducer is a polyanal acid special water reducer, the solid content of which is 45% and the water reduction rate is ≥35%.

[0079] In one embodiment of the present application, the particle size of the quartz sand ranges from 0.4 mm to 0.6 mm.

[0080] In one embodiment of the present application, the mass fractions of white silica fume are specifically: 0.1, 0.2, 0.3, 0.4, 0.5.

[0081] In one embodiment of the present application, the mass fractions of 325 mesh quartz powder are specifically: 0.2, 0.3, 0.4, 0.5.

[0082] In one embodiment of the present application, the mass fractions of quartz sand are specifically: 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5.

[0083] In one embodiment of the present application, the mass fraction of kaolin is specifically 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, and 0.18.

[0084] In one embodiment of the present application, the mass fraction of nano-CaO is specifically 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, or 0.08.

[0085] In one embodiment of the present application, the mass fraction of nano-Na2O is specifically: 0.01, 0.02, 0.03, 0.04.

[0086] In one embodiment of the present application, the mass fraction of calcium carbonate is specifically: 0.02, 0.03, 0.04, 0.05, 0.06.

[0087] In one embodiment of the present application, the mass fractions of the defoaming agent are specifically: 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08.

[0088] In one embodiment of the present application, the mass fractions of the water reducer are specifically: 0.01, 0.02, 0.03, 0.04, 0.045.

[0089] In one embodiment of the present application, the mass fraction of the synthetic fiber is specifically 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, or 0.10.

[0090] In one embodiment of the present application, the mass fractions of titanium dioxide are specifically 0.003, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, and 0.12.

[0091] In one embodiment of the present application, the mass fraction of water is specifically: 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22.

[0092] It should be noted that the decorative cement composite material provided by the present application is based on nanofiber reinforcement and toughening, and the structural components are prepared according to the structural form of the product and the specification requirements. The integrity of the structural product can be improved, and the structure is crack-resistant, high-strength, thin and light, and the structure has the purpose of high strength and high toughness. On the other hand, the use of white silicate cement and the addition of titanium dioxide can have a whitening effect, so that the basic color of the cement-based nanocomposite material is close to white, which is convenient for obtaining various color effects. The addition of color water or color pigments can obtain the corresponding decorative colors.

[0093] In addition, nano Na2O can fill coarse aggregate, increase density and improve compressive strength. The color of the material product can be diversified and customized according to customer needs. The color of various colors is prepared by a fully automatic color mixing machine for trial matching, and the color difference of the material is ensured to be 98% basically consistent. Adding nano Cao, since the nano particles are mainly dispersed in submicron-sized silica fume, in addition to filling the gaps between silica fume particles and improving density, it can also react with silica fume to generate hydrated calcium silicate. In addition to increasing the density of cement stone, the addition of calcium carbonate can also promote the hydration reaction of silicate minerals in cement and increase the toughness of cement. 325 mesh quartz powder is mainly used to fill coarse aggregate quartz sand, increase the density of the structure and improve the compressive strength. The defoamer can mainly improve the compressive strength and toughness of the structure, with a smooth and delicate surface, no bubbles, and the liquid is not easy to penetrate into the structure, affecting the decorative effect.

[0094] Based on the above-mentioned raw materials and corresponding weight parts, a specific technical solution is provided below for illustration. The raw materials and corresponding weight parts are shown in Table 1.

[0095] Table 1 - Preparation raw materials and corresponding mass parts

[0096]

[0097]

[0098] The decorative cement composite material provided by the present invention can reduce the cost of repeated construction and maintenance, improve the efficiency, and realize an artistic product integrating materials, structure, and decoration. The dead weight of the structure is reduced, and it can be used to decorate kitchens, toilets, stairs, and special structures on indoor non-load-bearing walls. It can save space and area, and also play a role in sound insulation. Both sides of the wall panels can achieve the same beauty as marble, and can also play a waterproof and heat-insulating role. It can achieve permanent decoration without repeated decoration, and the maintenance cost is low and convenient. If the wall panels are polluted, the surface layer can be removed by polishing to eliminate surface defects and stains. In some special structures, for example, walls, windows and doors, and decorative panels, the shape and color diversification are completed at one time, which solves the problem of repeated construction, that is, it increases the full life cycle of the product and saves the cost.

[0099] In a specific embodiment, the decorative cement composite material provided by the present invention is applied to outdoor structures, such as assembled bridges, sidewalk slabs and blind slabs, flower beds, and road extension stones. The structure and surface are solved at one time, and the color can be diversified. The structure is light and heavy, and the large-span structure is improved. It can also reduce the problem of traffic jams in the city and construction noise. It is prefabricated in the factory and assembled on site. The on-site assembly time is short, which means it is beautiful and maintenance-free. It can also be customized according to user needs.

[0100] The embodiment of the present application also provides a preparation method, which is applied to the above-mentioned decorative cement composite material, and the preparation method includes: stirring and mixing the raw materials according to the mass ratio, and pouring the mixture into a mold to form it, and demolding and curing it after hardening.

[0101] refer to Figure 1 In one embodiment of the present application, the preparation method specifically includes step 101a, step 102a, step 104a, step 105a, step 106a, and step 107a.

[0102] Step 101a, white silicate cement, white silica fume, nano-CaO, calcium carbonate, kaolin, and defoaming agent are mixed and stirred uniformly in sequence according to the mass ratio.

[0103] Step 102a, adding 325 mesh quartz powder to the uniformly stirred powder according to the mass ratio, and then adding quartz sand, nano-Na2O and titanium dioxide and stirring evenly.

[0104] Step 104a, adding water reducing agent and water according to the mass ratio, and stirring evenly until the mixture is fluidized;

[0105] Step 105a, after the materialization, continue to stir while uniformly adding the synthetic fibers to stir and disperse them uniformly;

[0106] Step 106a, pouring the uniformly stirred mixture into a mold, removing bubbles and forming by vibrating and vacuuming, and demoulding after hardening;

[0107] Step 107a, steam curing the hardened product at 60°C-80°C for 2-4 days.

[0108] It should be noted that the purpose of vacuuming is to allow the bubbles in the mixture to be discharged from the mixture as much as possible under the action of negative pressure, and the bubbles are removed by vibration and formed, and demolded after hardening. Through the above preparation method, an integrated building decoration structure can be produced. For example, a decorative building integrated kitchen, bathroom, staircase partition board, decorative board.

[0109] In one embodiment of the present application, pigments are added to the raw materials during the mixing process to generate the desired decorative color on the basis of white.

[0110] refer to Figure 2 In one embodiment of the present application, the preparation method specifically includes steps 101b to 107b.

[0111] Step 101b, white silicate cement, white silica fume, nano-CaO, calcium carbonate, kaolin, and defoaming agent are mixed and stirred uniformly in sequence according to the mass ratio.

[0112] Step 102b, adding 325 mesh quartz powder to the uniformly stirred powder according to the mass ratio, and then adding quartz sand, nano-Na2O, and titanium dioxide and stirring evenly.

[0113] Step 103b, adding the prepared color pigment in portions and stirring evenly.

[0114] Step 104b, adding water reducing agent and water according to the mass ratio, and stirring evenly until the mixture is fluidized.

[0115] Step 105b, after the fluidization, continue stirring while adding the synthetic fibers uniformly and stir to disperse them uniformly.

[0116] Step 106b, pouring the evenly stirred mixture into a mold, removing bubbles and shaping it by vibrating and vacuuming, and demoulding it after hardening.

[0117] Step 107b, steam curing the hardened product at 60°C-80°C for 2-4 days.

[0118] The embodiments of this application are Figure 1 On the basis of the steps of the corresponding preparation method, step 103b is added, that is, adding the prepared color pigment in portions and stirring evenly, and the pigment is added to obtain various colors required by users.

[0119] Based on the above preparation method, an embodiment of the present application also provides a building decoration structure, which is manufactured using the above preparation method.

[0120] This application improves the performance of existing active nano inorganic composite materials, so that they can be applied to decorative structures and improve the shortcomings of existing decorative structures. Compared with existing active nano inorganic composite materials, the decorative cement composite material provided by this application has the following advantages:

[0121] First, the decorative cement composite material provided by the present application adopts white silicate cement, and the addition of titanium dioxide can achieve a whitening effect, so that the basic color of the cement-based nanocomposite material is close to white, which is convenient for obtaining various color effects.

[0122] Second, it does not contain steel fibers, does not rust, and has better durability.

[0123] Third, the use of defoaming agent reduces bubbles, and the surface finish is high after construction.

[0124] When the decorative cement composite material provided by the present application is used for decoration, an integrated structure can be realized. Only one construction is required to form an integrated decorative structure, which replaces the main structure and outer layer decoration of the existing decoration, overcomes the problem of premature aging of the outer layer decorative material in the existing decorative structure, does not have the problem of the existing outer layer decoration falling off, eliminates safety hazards, and achieves lower costs, less space occupation, less weight, and higher strength. In addition, when the decorative cement composite material of the present application is used for decoration, its decorative structure is maintenance-free, and surface defects can be eliminated by removing a layer of surface material.

[0125] In the above embodiments of the present application, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, please refer to the relevant description of other embodiments.

[0126] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. It should be noted that the terms used here are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, work, devices, components and / or combinations thereof.

[0127] The specific embodiments described herein are merely examples of the spirit of the present application. A person skilled in the art of the present application may make various modifications or additions to the specific embodiments described or replace them in a similar manner, but this will not deviate from the spirit of the present application or exceed the scope defined by the attached claims.

Claims

1. A decorative cement composite material, characterized in that: The preparation raw materials and corresponding weight parts of the decorative cement composite material are as follows: White Portland cement: 1.0; White silica fume: 0.1 - 0.5; 325 mesh quartz powder: 0.2 - 0.5; Quartz sand: 0.6-1.5; Kaolin: 0.05-0.18; Nano-CaO: 0.02-0.08; Nano Na2O: 0.01-0.04; Calcium carbonate: 0.02-0.06; Defoamer: 0.005-0.08; Water reducing agent: 0.01–0.045; Synthetic fiber: 0.02-0.1; Titanium dioxide: 0.003-0.12; Water: 0.16-0.

22.

2. The decorative cement composite material according to claim 1, characterized in that: The decorative cement composite material further comprises a pigment.

3. The decorative cement composite material according to claim 1, characterized in that: The water reducing agent is a special poly-angiate water reducing agent with a solid content of 45% and a water reducing rate of ≥35%.

4. The decorative cement composite material according to claim 1, characterized in that: The particle size of the quartz sand is in the range of 0.4 mm to 0.6 mm.

5. The decorative cement composite material according to claim 1, characterized in that: The specific weight percentages of the white silica fume are: 0.1, 0.2, 0.3, 0.4, 0.5; The mass fractions of the 325 mesh quartz powder are specifically: 0.2, 0.3, 0.4, 0.5; The mass fractions of the quartz sand are specifically: 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5; The mass fractions of the kaolin are specifically: 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18; The specific mass fractions of the nano-CaO are: 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08; The specific mass fractions of the nano-Na2O are: 0.01, 0.02, 0.03, 0.04; The specific mass fractions of calcium carbonate are: 0.02, 0.03, 0.04, 0.05, 0.06; The mass parts of the defoaming agent are specifically: 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08; The mass fractions of the water reducing agent are specifically: 0.01, 0.02, 0.03, 0.04, 0.045; The mass fractions of the synthetic fibers are specifically: 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10; The specific mass fractions of the titanium dioxide are: 0.003, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12; The specific mass parts of water are: 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, and 0.

22.

6. A preparation method, characterized in that: The preparation method is applied to the decorative cement composite material according to any one of claims 1 to 5, comprising: The raw materials are stirred and mixed according to the mass ratio, and the mixture is poured into a mold for molding. After hardening, it is demoulded and cured.

7. The preparation method according to claim 6, characterized in that: During the mixing process of the raw materials, the pigment is added and stirred.

8. The preparation method according to claim 6, characterized in that: The preparation method specifically comprises the steps of: Step 101a, white silicate cement, white silica fume, nano-CaO, calcium carbonate, kaolin, and defoamer are mixed and stirred in sequence according to the mass ratio; Step 102a, adding 325 mesh quartz powder to the uniformly stirred powder according to the mass ratio, and then adding quartz sand, nano-Na2O, and titanium dioxide and stirring evenly; Step 104a, adding water reducing agent and water according to the mass ratio, and stirring evenly until the mixture is fluidized; Step 105a, after the materialization, continue to stir while uniformly adding the synthetic fiber, stirring to evenly disperse; Step 106a, pouring the uniformly stirred mixture into a mold, removing bubbles and forming by vibrating and vacuuming, and demoulding after hardening; Step 107a, steam curing the hardened product at 60°C-80°C for 2-4 days.

9. The preparation method according to claim 7, characterized in that: The preparation method specifically comprises the steps of: Step 101b, mixing white silicate cement, white silica fume, nano-CaO, calcium carbonate, kaolin, and defoamer in sequence according to the mass ratio and stirring evenly; Step 102b, adding 325 mesh quartz powder to the uniformly stirred powder according to the mass ratio, and then adding quartz sand, nano-Na2O, and titanium dioxide and stirring evenly; Step 103b, adding the prepared color pigment in portions and stirring evenly; Step 104b, adding water reducing agent and water according to the mass ratio, and stirring evenly until the mixture is fluidized; Step 105b, after the materialization, continue to stir while uniformly adding the synthetic fibers to stir and disperse them uniformly; Step 106b, pouring the uniformly stirred mixture into a mold, removing bubbles and forming by vibrating and vacuuming, and demoulding after hardening; Step 107b, steam curing the hardened product at 60°C-80°C for 2-4 days.

10. A building decoration structure, characterized in that: The architectural decoration structure is manufactured using the preparation method described in any one of claims 6 to 9.