Preparation method of solid spherical aluminum oxide granulation powder
By using specific anionic and cationic surfactants to adjust the dispersibility of alumina slurry, the problem of manufacturing completely solid spherical alumina granules was solved, achieving a production effect that is simple to operate and easy to control, and improving the fluidity and morphology control of the slurry.
Patent Information
- Application Number
- CN202410952795.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Existing technologies make it difficult to manufacture completely solid spherical alumina granules, and the manufacturing equipment is complex and production control is difficult.
Solid spherical alumina granules were prepared by adjusting the dispersibility of alumina slurry with specific anionic and cationic surfactants and by ball milling and spray granulation.
It achieves complete solid spheroidization of alumina granulated powder, reduces the requirements for manufacturing equipment and the difficulty of control, and improves the yield stress and thixotropy of alumina slurry.
Smart Images

Figure CN118908703A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic materials, and in particular to a method for preparing solid spherical alumina granulated powder. Background Art
[0002] Alumina ceramics have the characteristics of high strength, good corrosion resistance, and excellent insulation, and are widely used in new energy vehicles, LEDs, semiconductors, etc. The dry pressing process has the advantages of high production efficiency, high degree of automation, and low production cost, and is one of the main processes for manufacturing alumina ceramic parts.
[0003] Since alumina powder is a ridged raw material, it has problems such as low bulk density and poor fluidity, and cannot be directly used in the dry pressing process. Therefore, before dry pressing, the alumina powder needs to be prepared into a slurry, and then the alumina slurry is dried by a spray granulation method to form an alumina granulated powder with good fluidity. There are generally three types of morphology of alumina granulated powder: solid sphere, apple shape and hollow sphere. Among them, the solid spherical alumina granulated powder has the best fluidity and the largest bulk density. It is difficult to produce a completely solid spherical alumina granulated powder in actual production. Chinese invention patent CN104150883B discloses a method for preparing alumina granulated powder, and proposes to use a centrifugal-pressure combined method to manufacture solid granulated powder. However, this method has problems such as complex manufacturing equipment structure, difficult production control, and a certain proportion of hollow balls in the product. Therefore, finding a method for manufacturing alumina granulated powder that is simple to control and completely solid and spherical is a problem that the entire industry urgently needs to solve. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing solid spherical alumina granulated powder. By adjusting the dispersibility of alumina slurry, the alumina granulated powder can be completely solid spheroidized, with simple requirements on manufacturing equipment and low control difficulty.
[0005] In order to achieve the above object, the solution of the present invention is:
[0006] A method for preparing solid spherical alumina granulated powder comprises the following steps:
[0007] Step 1: According to the proportion, 50 wt% to 60 wt% of alumina powder, 3 wt% to 6 wt% of a sintering aid, 0.2 wt% to 0.6 wt% of anionic surfactant dispersant and 35 wt% to 45 wt% of deionized water are first put into a ball mill for ball milling and dispersion to obtain alumina slurry A;
[0008] Step 2: Add the binder and the plasticizer to the alumina slurry A according to the ratio, and perform ball milling to obtain the alumina slurry B;
[0009] The amount of the binder added is 1.0% to 3.0% of the mass of the alumina powder, and the amount of the plasticizer added is 0.5% to 3.0% of the mass of the alumina powder.
[0010] Step 3, according to the ratio, a cationic surfactant dispersant is added to the alumina slurry B, and the alumina slurry C is obtained by ball milling again, wherein the amount of the cationic surfactant dispersant added is 0.05% to 0.15% relative to the mass of the alumina powder;
[0011] Step 4: finally, spray granulation is performed on the alumina slurry C, and the conditions of the spray granulation are: air inlet temperature: 250-280° C., air outlet temperature: 100-110° C., and pressure in the tower: -10-50 Pa, to obtain the solid spherical alumina granulated powder;
[0012] In step 1, the molecular structure of the anionic surfactant dispersant is shown in Formula I:
[0013]
[0014] In formula I, R1 and R2 are H, COOH, COO - Na + 、COO - K + 、COO - NH + 4. COO - N + H(CH3)2CH2CH2OH、COO - N + H(CH2CH3)3, R3 is one of butyl, isobutyl, isooctyl and isobornyl, R4 is one of H and methyl; a=0.1-0.4, b=0.16-0.67, c=0.23-0.44, n=3-14, wherein the values of a, b and c are the molar ratios of the corresponding monomers;
[0015] In step 3, the molecular structure of the cationic surfactant dispersant is shown in II:
[0016]
[0017] In Formula II, R1, R2 and R5 are respectively one of H and methyl, R3 is one of butyl, isobutyl, isooctyl and isobornyl, and R4 is one of H and methyl;
[0018] R6 is and one of CH3COOCH2CH(OH)CH2-;
[0019] a=0.1~0.4,b=0.16~0.67,c=0.23~0.44,n=3~14,wherein the values of a, b and c are the molar ratios of the corresponding monomers.
[0020] In step 1, the particle size of the alumina powder is 2.0-3.0 μm, and the sintering aid includes 15wt%-45wt% SiO2, 15wt%-23wt% CaCO3 and 33wt%-70wt% talc.
[0021] In step 1, the rotation speed of the ball mill is 20 to 35 rpm, and the ball milling time is 12 to 24 hours.
[0022] In step 2, the binder is one of polyvinyl alcohol and water-based acrylic resin, and the plasticizer is one or both of polyethylene glycol and glycerol.
[0023] In step 2, the rotation speed of the ball mill is 20 to 35 rpm, and the ball milling time is 2 to 6 hours; in step 3, the rotation speed of the ball mill is 20 to 35 rpm, and the ball milling time is 1 to 5 hours.
[0024] In step 1, the preparation method of the anionic surfactant dispersant is as follows: first, 5 to 30 parts of maleic anhydride or acrylic acid monomer, 23 to 64 parts of polyethylene glycol monoether acrylate, 20 to 60 parts of (methyl) acrylate monomer, 0.5 to 5 parts of initiator and 60 to 140 parts of solvent are added to a container in sequence, and stirred evenly at room temperature to obtain a uniform mixed solution; then, 30 to 60 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 75 to 95° C., and the temperature is kept for 20 to 90 minutes, and then the remaining mixed solution is added dropwise within 0.5 to 4 hours, and the temperature is kept for 1 to 3 hours, and then 30 to 100 parts of deionized water are added to cool to below 40° C., and 5 to 40 parts of a neutralizing agent are added for a neutralization reaction. After the reaction is performed for 0.5 to 1 hour, the solvent is removed by reduced pressure distillation to obtain the anionic surfactant dispersant.
[0025] The (meth)acrylate monomer is one of butyl (meth)acrylate, isobutyl (meth)acrylate, isooctyl (meth)acrylate, and isobornyl (meth)acrylate; the initiator is one of azobisisobutyronitrile and ammonium persulfate; the solvent is one or more of ethyl acetate, isopropanol, water, toluene, propylene glycol methyl ether, and butyl acetate; and the neutralizing agent is one of sodium hydroxide, potassium hydroxide, N,N-dimethylethanolamine, triethylamine, ammonia water, and ammonium hydroxide.
[0026] In step 3, the preparation method of the cationic surfactant dispersant is as follows: first, 5 to 40 parts of cationic monomer, 23 to 64 parts of polyethylene glycol monoether acrylate, 20 to 60 parts of (meth) acrylate monomer, 0.5 to 5 parts of initiator and 60 to 140 parts of solvent are added to a container, and stirred evenly at room temperature to obtain a uniform mixed solution; then, 30 to 60 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 75 to 95° C., and the mixture is kept warm for 20 to 90 minutes, and then the remaining mixed solution is added dropwise within 0.5 to 4 hours, and the mixture is kept warm for 1 to 3 hours, and then the temperature is lowered to below 60° C., and then 5 to 40 parts of chloride are added, and the mixture is kept warm for 0.5 to 2 hours, and then 20 to 50 parts of deionized water are added to lower the temperature to below 40° C., and finally 5 to 40 parts of fatty acid are added, and after reacting for 0.5 to 1 hour, the solvent is removed by reduced pressure distillation to obtain the cationic surfactant dispersant.
[0027] The cationic monomer is one of dimethylaminoethyl (meth)acrylate, N,N-dimethylacrylamide and acrylamide; the (meth)acrylate monomer is one of butyl (meth)acrylate, isobutyl (meth)acrylate, isooctyl (meth)acrylate and isobornyl (meth)acrylate; the initiator is one of azobisisobutyronitrile and ammonium persulfate; the solvent is one or more of ethyl acetate, isopropanol, water, toluene, propylene glycol methyl ether and butyl acetate; the chloride is one of methyl chloroacetate, epichlorohydrin and chloroacetic acid; the fatty acid is one of acetic acid, lauric acid and stearic acid.
[0028] After adopting the above technical scheme, the present invention provides a method for preparing a solid spherical alumina granulated powder, first adding a specific anionic surfactant dispersant to disperse and mix the alumina powder and the sintering aid, then adding a specific cationic surfactant dispersant to neutralize the surface charge of the anionic surfactant dispersant to obtain an alumina slurry, and finally spray granulating to obtain a solid spherical alumina granulated powder. Through this preparation method, the uniformity of the mixing of the alumina powder and the sintering aid can be ensured, and the yield stress and thixotropy of the alumina slurry can be improved, so that the alumina slurry presents a solid sphere after granulation. In general, the present invention adjusts the dispersibility of the alumina slurry by using two dispersants with opposite characteristics, so as to achieve complete solid spheroidization of the alumina granulated powder, and has simple requirements for manufacturing equipment and low control difficulty. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a SEM scan of the solid spherical alumina granulated powder prepared in Example 7;
[0030] Figure 2 This is a SEM scan of the ordinary spherical alumina granulated powder prepared in Comparative Example 1. DETAILED DESCRIPTION
[0031] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.
[0032] 1. Preparation of solid spherical alumina granulated powder
[0033] (1) Preparation of anionic surfactant dispersants
[0034] Example 1
[0035] First, 25 parts of maleic anhydride, 35 parts of polyethylene glycol monoether acrylate, 30 parts of (methyl) acrylate isobornyl, 2 parts of azobisisobutyronitrile and 100 parts of propylene glycol methyl ether are added to a three-necked flask in sequence, and stirred evenly at room temperature to obtain a uniform mixed solution; then 30 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 80°C within 30 minutes, and the temperature is kept for 30 minutes, and then the remaining mixed solution is added dropwise within 3 hours, and the temperature is kept for 3 hours, and then 50 parts of deionized water are added to cool to below 40°C, and 30 parts of ammonium hydroxide are added for neutralization, and after reacting for 30 minutes, the solvent is removed by reduced pressure distillation to obtain the anionic surfactant dispersant.
[0036] The molecular structure of the anionic surfactant dispersant is shown in Formula III:
[0037]
[0038] Among them, a=0.22~0.30, b=0.40~0.46, c=0.35~0.41, and n=7~9.
[0039] Example 2
[0040] First, 20 parts of acrylic acid, 40 parts of polyethylene glycol monoether acrylate, 30 parts of (methyl) acrylate isobornyl, 1.5 parts of azobisisobutyronitrile and 90 parts of ethyl acetate are added to a three-necked flask in sequence, and stirred evenly at room temperature to obtain a uniform mixed solution; then 30 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 80°C within 30 minutes, and the temperature is kept for 30 minutes, and then the remaining mixed solution is added dropwise within 2.5 hours, and the temperature is kept for 1 hour, and then 30 parts of deionized water are added to dissolve and the temperature is lowered to below 40°C, and 20 parts of N,N-dimethylethanolamine are added for neutralization, and the solvent is removed by reduced pressure distillation to obtain the anionic surfactant dispersant.
[0041] The molecular structure of the anionic surfactant dispersant is shown in Formula IV:
[0042]
[0043] Among them, a=0.20~0.28, b=0.50~0.56, c=0.35~0.41, and n=8.
[0044] Example 3
[0045] First, 30 parts of acrylic acid, 20 parts of polyethylene glycol monoether acrylate, 40 parts of butyl (meth)acrylate, 2.5 parts of azobisisobutyronitrile and 100 parts of ethyl acetate are added to a three-necked flask in sequence, and stirred evenly at room temperature to obtain a uniform mixed solution; then 30 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 75°C within 30 minutes, and the temperature is kept for 30 minutes, and then the remaining mixed solution is added dropwise within 3 hours, and the temperature is kept for 3 hours, and then 50 parts of deionized water are added to dissolve and the temperature is lowered to below 40°C, 20 parts of N,N-dimethylethanolamine are added for neutralization, and the solvent is removed by reduced pressure distillation to obtain the anionic surfactant dispersant.
[0046] The molecular structure of the anionic surfactant dispersant is shown in Formula V:
[0047]
[0048] Among them, a=0.35~0.40, b=0.50~0.56, c=0.35~0.41, and n=8.
[0049] (2) Preparation of cationic surfactant dispersants
[0050] Example 4
[0051] First, 30 parts of N,N-dimethylacrylamide, 50 parts of polyethylene glycol monoether acrylate, 20 parts of (methyl) acrylate isobornyl, 2 parts of azobisisobutyronitrile and 100 parts of propylene glycol methyl ether are added to a three-necked flask, and stirred evenly at room temperature to obtain a uniform mixed solution; then 30 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 80°C within 30 minutes, and the temperature is kept for 30 minutes, and then the remaining mixed solution is dripped within 3 hours, and the solvent is removed after keeping the temperature for 3 hours, and then the temperature is lowered to below 60°C, and 30 parts of epichlorohydrin are added, and the temperature is kept for 1 hour, and then 50 parts of deionized water are added to lower the temperature to below 40°C, and then 30 parts of acetic acid are added to react for half an hour, and the solvent is removed by reduced pressure distillation to obtain the cationic surfactant dispersant.
[0052] The molecular structure of the cationic surfactant dispersant is shown in VI:
[0053]
[0054] Among them, a=0.27~0.33, b=0.47~0.53, c=0.36~0.40, n=7~9.
[0055] Example 5
[0056] First, 30 parts of acrylamide, 40 parts of polyethylene glycol monoether acrylate, 30 parts of (methyl) acrylate isobornyl, 2 parts of azobisisobutyronitrile and 100 parts of propylene glycol methyl ether are added to a three-necked flask, and stirred evenly at room temperature to obtain a uniform mixed solution; then 30 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, and the temperature is raised to 90° C. within 30 minutes, and then the remaining mixed solution is dripped within 3 hours, and the temperature is kept for 2 hours, and then the temperature is lowered to below 60° C., and 32 parts of epichlorohydrin are added, and the temperature is kept for 1 hour. Then 40 parts of deionized water are added to cool to below 40° C., and then 32 parts of acetic acid are added to react for half an hour, and the solvent is removed by reduced pressure distillation to obtain the cationic surfactant dispersant.
[0057] The molecular structure of the cationic surfactant dispersant is shown in VII:
[0058]
[0059]
[0060] Among them, a=0.27~0.33, b=0.47~0.53, c=0.36~0.40, n=7~9.
[0061] (3) Preparation of solid spherical alumina granulated powder
[0062] Example 6
[0063] A method for preparing solid spherical alumina granulated powder comprises the following steps:
[0064] Step 1: According to the ratio, 60 wt% of alumina powder, 4.5 wt% of sintering aid, 0.5 wt% of anionic surfactant dispersant prepared in Example 1 and 35 wt% of deionized water are put into a horizontal ball mill for ball milling dispersion at a speed of 30 rpm for 18 h to obtain alumina slurry A;
[0065] Step 2: Add polyvinyl alcohol and polyethylene glycol to alumina slurry A according to the ratio, and perform ball milling at a speed of 30 rpm for 6 hours to obtain alumina slurry B;
[0066] The amount of polyvinyl alcohol added is 1.0% of the mass of the aluminum oxide powder, and the amount of polyethylene glycol added is 1.0% of the mass of the aluminum oxide powder.
[0067] Step 3, according to the ratio, the cationic surfactant dispersant prepared in Example 4 is then added to the alumina slurry B, and the ball milling is dispersed again, the ball milling speed is 30 rpm, and the ball milling is performed for 3 hours to obtain an alumina slurry C, wherein the amount of the cationic surfactant dispersant added is 0.15% of the mass of the alumina powder;
[0068] Step 4: Finally, a centrifugal spray granulation tower is used to spray granulate the alumina slurry C. The spray granulation conditions are: inlet air temperature: 250°C, outlet air temperature: 100°C, and pressure in the tower: 30Pa to obtain the solid spherical alumina granulated powder.
[0069] In step 1, the particle size of the alumina powder is 2.0-3.0 μm, and the sintering aid includes 30 wt % SiO 2 , 20 wt % CaCO 3 and 50 wt % talc.
[0070] Example 7
[0071] A method for preparing solid spherical alumina granulated powder comprises the following steps:
[0072] Step 1: According to the ratio, 55 wt% of alumina powder, 4.4 wt% of sintering aid, 0.6 wt% of anionic surfactant dispersant prepared in Example 2 and 40 wt% of deionized water are put into a horizontal ball mill for ball milling dispersion at a speed of 20 rpm for 12 h to obtain alumina slurry A;
[0073] Step 2: Add water-based acrylic resin and polyethylene glycol to alumina slurry A according to the ratio, and perform ball milling at a speed of 20 rpm for 4 hours to obtain alumina slurry B;
[0074] The amount of waterborne acrylic resin added is 2.0% of the mass of aluminum oxide powder, and the amount of polyethylene glycol added is 2.0% of the mass of aluminum oxide powder.
[0075] Step 3, according to the ratio, the cationic surfactant dispersant prepared in Example 5 is then added to the alumina slurry B, and the ball milling is dispersed again, the ball milling speed is 20 rpm, and the ball milling is performed for 1 hour to obtain an alumina slurry C, wherein the amount of the cationic surfactant dispersant added is 0.10% of the mass of the alumina powder;
[0076] Step 4: Finally, a centrifugal spray granulation tower is used to spray granulate the alumina slurry C. The spray granulation conditions are: inlet air temperature: 280°C, outlet air temperature: 110°C, and pressure in the tower: 50Pa to obtain the solid spherical alumina granulated powder.
[0077] In step 1, the particle size of the alumina powder is 2.0-3.0 μm, and the sintering aid includes 32 wt % SiO 2 , 28 wt % CaCO 3 and 40 wt % talc.
[0078] Example 8
[0079] A method for preparing solid spherical alumina granulated powder comprises the following steps:
[0080] Step 1: According to the ratio, 50 wt% of alumina powder, 4.5 wt% of sintering aid, 0.5 wt% of anionic surfactant dispersant prepared in Example 3 and 45 wt% of deionized water are put into a horizontal ball mill for ball milling dispersion at a speed of 35 rpm for 24 hours to obtain alumina slurry A;
[0081] Step 2: Add water-based acrylic resin and polyethylene glycol to alumina slurry A according to the ratio, and perform ball milling at a speed of 35 rpm for 2 h to obtain alumina slurry B;
[0082] The amount of waterborne acrylic resin added is 3.0% of the mass of aluminum oxide powder, and the amount of polyethylene glycol added is 3.0% of the mass of aluminum oxide powder.
[0083] Step 3, according to the ratio, the cationic surfactant dispersant prepared in Example 5 is then added to the alumina slurry B, and the ball milling is dispersed again, the ball milling speed is 35 rpm, and the ball milling is performed for 5 hours to obtain an alumina slurry C, wherein the amount of the cationic surfactant dispersant added is 0.10% of the mass of the alumina powder;
[0084] Step 4: Finally, a centrifugal spray granulation tower is used to spray granulate the alumina slurry C. The spray granulation conditions are: inlet air temperature: 250°C, outlet air temperature: 100°C, and pressure in the tower: 10Pa to obtain the solid spherical alumina granulated powder.
[0085] In step 1, the particle size of the alumina powder is 2.0-3.0 μm, and the sintering aid includes 30 wt % SiO 2 , 20 wt % CaCO 3 and 50 wt % talc.
[0086] Comparative Example 1
[0087] A method for preparing alumina granulated powder comprises the following steps:
[0088] Step 1: According to the ratio, 55 wt% alumina powder, 4.4 wt% sintering aid and 40.6 wt% deionized water are first put into a horizontal ball mill for ball milling dispersion at a speed of 20 rpm for 12 hours to obtain alumina slurry A;
[0089] Step 2: Add water-based acrylic resin and polyethylene glycol to alumina slurry A according to the ratio, and perform ball milling at a speed of 20 rpm for 4 hours to obtain alumina slurry B;
[0090] The amount of waterborne acrylic resin added is 2.0% of the mass of aluminum oxide powder, and the amount of polyethylene glycol added is 2.0% of the mass of aluminum oxide powder.
[0091] Step 3: Finally, a centrifugal spray granulation tower is used to spray granulate the alumina slurry B. The spray granulation conditions are: inlet air temperature: 280°C, outlet air temperature: 100°C, and pressure in the tower: 50Pa to obtain the alumina granulated powder.
[0092] In step 1, the particle size of the alumina powder is 2.0-3.0 μm, and the sintering aid includes 32 wt % SiO 2 , 28 wt % CaCO 3 and 40 wt % talc.
[0093] Comparative Example 2
[0094] A method for preparing alumina granulated powder comprises the following steps:
[0095] Step 1: According to the ratio, 55 wt% of alumina powder, 4.4 wt% of sintering aid, 0.6 wt% of anionic surfactant dispersant prepared in Example 2 and 40 wt% of deionized water are put into a horizontal ball mill for ball milling dispersion at a speed of 20 rpm for 12 h to obtain alumina slurry A;
[0096] Step 2: Add water-based acrylic resin and polyethylene glycol to alumina slurry A according to the ratio, and perform ball milling at a speed of 20 rpm for 4 hours to obtain alumina slurry B;
[0097] The amount of waterborne acrylic resin added is 2.0% of the mass of aluminum oxide powder, and the amount of polyethylene glycol added is 2.0% of the mass of aluminum oxide powder.
[0098] Step 3: Finally, a centrifugal spray granulation tower is used to spray granulate the alumina slurry B. The spray granulation conditions are: inlet air temperature: 280°C, outlet air temperature: 110°C, and pressure in the tower: 50Pa to obtain the solid spherical alumina granulated powder.
[0099] In step 1, the particle size of the alumina powder is 2.0-3.0 μm, and the sintering aid includes 32 wt % SiO 2 , 28 wt % CaCO 3 and 40 wt % talc.
[0100] In the above embodiments and comparative examples, the raw materials used were all purchased from the market.
[0101] 2. Morphology test
[0102] The morphology of the alumina granulated powder prepared in Example 7 and Comparative Example 1 was obtained by scanning electron microscope TM-4000plus produced by Hitachi, Japan, under the following conditions: test voltage: 15 kV, magnification: 200x. Figure 1 and Figure 2 As shown, the solid spheroidization of the alumina granulated powder prepared in Example 7 is more complete, and the alumina granulated powder prepared in Comparative Example 1 is more hemispherical.
[0103] 3. Performance testing
[0104] (1) Test method
[0105] The yield stress of the alumina slurry obtained in step 3 was measured using an Anton Paar MCR102e rheometer under the following measurement conditions: rotor diameter: 50 mm, angle: 1°, temperature: 25°C, shear rate: 0.01-1000 s -1 , the casson plot model is used to simulate the curve and obtain the slurry yield stress.
[0106] Thixotropy test method of slurry:
[0107] The yield stress of the alumina slurry obtained in step 3 was measured using an Anton Paar MCR102e rheometer under the following measurement conditions: rotor diameter: 25 mm, angle: 1°, temperature: 25°C, shear rate: 0.01-1000 s -1 , using the formula: Thixotropy = 5s -1 Lower viscosity / 50s -1 The viscosity is reduced to obtain thixotropy of the alumina slurry.
[0108] (2) Test results
[0109] The test results are shown in Table 1, which show that the yield stress and thixotropy of the alumina slurry after adding two dispersants with opposite characteristics are good.
[0110] Table 1 Performance test results of alumina slurry
[0111]
[0112]
[0113] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.
Claims
1. A method for preparing solid spherical alumina granulated powder, characterized in that: The following steps are involved: Step 1: According to the proportion, 50 wt% to 60 wt% of alumina powder, 3 wt% to 6 wt% of a sintering aid, 0.2 wt% to 0.6 wt% of anionic surfactant dispersant and 35 wt% to 45 wt% of deionized water are first put into a ball mill for ball milling and dispersion to obtain alumina slurry A; Step 2: Add the binder and the plasticizer to the alumina slurry A according to the ratio, and perform ball milling to obtain the alumina slurry B; The amount of the binder added is 1.0% to 3.0% of the mass of the alumina powder, and the amount of the plasticizer added is 0.5% to 3.0% of the mass of the alumina powder. Step 3, according to the ratio, a cationic surfactant dispersant is added to the alumina slurry B, and the alumina slurry C is obtained by ball milling again, wherein the amount of the cationic surfactant dispersant added is 0.05% to 0.15% relative to the mass of the alumina powder; Step 4: finally, spray granulation is performed on the alumina slurry C, and the conditions of the spray granulation are: air inlet temperature: 250-280° C., air outlet temperature: 100-110° C., and pressure in the tower: -10-50 Pa, to obtain the solid spherical alumina granulated powder; In step 1, the molecular structure of the anionic surfactant dispersant is shown in Formula I: In formula I, R1 and R2 are H, COOH, COO - Na + 、COO - K + 、COO - NH + 4. COO - N + H(CH3)2CH2CH2OH、COO - N + H(CH2CH3)3, R3 is one of butyl, isobutyl, isooctyl and isobornyl, R4 is one of H and methyl; a=0.1-0.4, b=0.16-0.67, c=0.23-0.44, n=3-14, wherein the values of a, b and c are the molar ratios of the corresponding monomers; In step 3, the molecular structure of the cationic surfactant dispersant is shown in II: In Formula II, R1, R2 and R5 are respectively one of H and methyl, R3 is one of butyl, isobutyl, isooctyl and isobornyl, R4 is one of H and methyl; R6 is and one of CH3COOCH2CH(OH)CH2-; a=0.1~0.4,b=0.16~0.67,c=0.23~0.44,n=3~14,wherein the values of a, b and c are the molar ratios of the corresponding monomers.
2. The method for preparing a solid spherical alumina granulated powder according to claim 1, characterized in that: In step 1, the particle size of the alumina powder is 2.0-3.0 μm, and the sintering aid includes 15wt%-45wt% SiO2, 15wt%-23wt% CaCO3 and 33wt%-70wt% talc.
3. The method for preparing a solid spherical alumina granulated powder according to claim 1, characterized in that: In step 1, the rotation speed of the ball mill is 20 to 35 rpm, and the ball milling time is 12 to 24 hours.
4. The method for preparing a solid spherical alumina granulated powder according to claim 1, characterized in that: In step 2, the binder is one of polyvinyl alcohol and water-based acrylic resin, and the plasticizer is one or both of polyethylene glycol and glycerol.
5. The method for preparing a solid spherical alumina granulated powder according to claim 1, characterized in that: In step 2, the rotation speed of the ball mill is 20 to 35 rpm, and the ball milling time is 2 to 6 hours; in step 3, the rotation speed of the ball mill is 20 to 35 rpm, and the ball milling time is 1 to 5 hours.
6. The method for preparing a solid spherical alumina granulated powder according to claim 1, characterized in that: In step 1, the preparation method of the anionic surfactant dispersant is as follows: first, 5 to 30 parts of maleic anhydride or acrylic acid monomer, 23 to 64 parts of polyethylene glycol monoether acrylate, 20 to 60 parts of (methyl) acrylate monomer, 0.5 to 5 parts of initiator and 60 to 140 parts of solvent are added to a container in sequence, and stirred evenly at room temperature to obtain a uniform mixed solution; then, 30 to 60 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 75 to 95° C., and the temperature is kept for 20 to 90 minutes, and then the remaining mixed solution is added dropwise within 0.5 to 4 hours, and the temperature is kept for 1 to 3 hours, and then 30 to 100 parts of deionized water are added to cool to below 40° C., and 5 to 40 parts of a neutralizing agent are added for neutralization reaction. After reacting for 0.5 to 1 hour, the solvent is removed by reduced pressure distillation to obtain the anionic surfactant dispersant.
7. The method for preparing a solid spherical alumina granulated powder according to claim 6, characterized in that: The (meth)acrylate monomer is one of butyl (meth)acrylate, isobutyl (meth)acrylate, isooctyl (meth)acrylate, and isobornyl (meth)acrylate; the initiator is one of azobisisobutyronitrile and ammonium persulfate; the solvent is one or more of ethyl acetate, isopropanol, water, toluene, propylene glycol methyl ether, and butyl acetate; and the neutralizing agent is one of sodium hydroxide, potassium hydroxide, N,N-dimethylethanolamine, triethylamine, ammonia water, and ammonium hydroxide.
8. The method for preparing a solid spherical alumina granulated powder according to claim 1, characterized in that: In step 3, the preparation method of the cationic surfactant dispersant is as follows: first, 5 to 40 parts of cationic monomer, 23 to 64 parts of polyethylene glycol monoether acrylate, 20 to 60 parts of (meth) acrylate monomer, 0.5 to 5 parts of initiator and 60 to 140 parts of solvent are added to a container, and stirred evenly at room temperature to obtain a uniform mixed solution; then, 30 to 60 parts of the mixed solution are added to a four-necked flask, and nitrogen is continuously introduced, the temperature is raised to 75 to 95° C., and the mixture is kept warm for 20 to 90 minutes, and then the remaining mixed solution is added dropwise within 0.5 to 4 hours, and the mixture is kept warm for 1 to 3 hours, and then the temperature is lowered to below 60° C., and then 5 to 40 parts of chloride are added, and the mixture is kept warm for 0.5 to 2 hours, and then 20 to 50 parts of deionized water are added to lower the temperature to below 40° C., and finally 5 to 40 parts of fatty acid are added, and after reacting for 0.5 to 1 hour, the solvent is removed by reduced pressure distillation to obtain the cationic surfactant dispersant.
9. The method for preparing a solid spherical alumina granulated powder according to claim 8, characterized in that: The cationic monomer is one of dimethylaminoethyl (meth)acrylate, N,N-dimethylacrylamide and acrylamide; the (meth)acrylate monomer is one of butyl (meth)acrylate, isobutyl (meth)acrylate, isooctyl (meth)acrylate and isobornyl (meth)acrylate; the initiator is one of azobisisobutyronitrile and ammonium persulfate; the solvent is one or more of ethyl acetate, isopropanol, water, toluene, propylene glycol methyl ether and butyl acetate; the chloride is one of methyl chloroacetate, epichlorohydrin and chloroacetic acid; the fatty acid is one of acetic acid, lauric acid and stearic acid.
Citation Information
Patent Citations
Preparation method of spherical catalyst carrier
CN103041868A
99%-above alumina granulating powder and preparation method thereof
CN105384428A
Dispersing agent and preparation method thereof
CN108912285A
Dispersible aluminum oxide as well as preparation method and application thereof
CN113213900A
Low-process-cost preparation method of solid spherical AT13 spraying feed
CN113248235A