Method for preparing yttrium aluminum oxide ceramic precursor

By introducing yttrium elements into the Al2O3 precursor system, adjusting the element ratio by polymer precursor method, high-performance YAG and Al2O3-YAG composite fibers are prepared, and environmental protection and mechanical properties in the preparation of YAG fibers in the prior art are solved. Problem, high temperature stability and high efficiency ceramic fiber preparation are achieved.

CN118908711APending Publication Date: 2024-11-08INST OF CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202310511193.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

It is difficult to prepare high-performance YAG fibers in the prior art. The spinning raw materials contain Cl elements and spinning additives, which is not conducive to the preparation of environmental protection and high-performance fibers. High-temperature sintering leads to an increase in grain size and affects the mechanical properties.

Method used

Yttrium element was introduced into the pure Al2O3 precursor system, and the proportion of Y and Al elements was adjusted by polymer precursor method, and the YAG precursor and Al2O3-YAG complex phase precursor were designed and synthesized, and yttrium aluminum oxidation was prepared by melt spinning and post-treatment processes. Continuous ceramic fibers can improve the stability of high-temperature grain size and high-temperature resistance.

Benefits of technology

A continuous ceramic fiber of yttrium aluminum oxide with excellent high temperature performance was prepared. The fiber's high-temperature grain size stability and high-temperature resistance were improved, and the ceramic yield reached 39%, which was suitable for composite materials in high-temperature oxidation environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908711A_ABST
    Figure CN118908711A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an yttrium aluminum oxide ceramic precursor. An aluminum source and a yttrium source are dissolved in an organic solvent according to a certain proportion, a complexing agent is adopted for conducting coordination stabilization on the mixed solution, then hydrolytic polycondensation is conducted, the spinning performance of a precursor is improved by adjusting a synthesis process according to different yttrium-aluminum element proportions, and then the yttrium-aluminum oxide continuous ceramic fiber composed of different crystal phases is prepared. The high-temperature grain size stability and the high-temperature resistance of the fiber are improved. The softening point of the yttrium aluminum oxide ceramic precursor is 110-180 DEG C, and the highest ceramic yield is 39%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite fiber materials, and in particular relates to a method for preparing a yttrium aluminum oxide ceramic precursor. Background Art

[0002] With the development of international aerospace industry, high-performance thermal protection materials have gradually become a research hotspot in the frontier field of national defense. Ceramic-based composite materials, as ideal materials for use in high-temperature extreme environments, are developing rapidly around the world. Yttrium aluminum garnet (YAG) is the only binary compound in the Y2O3-Al2O3 system that can exist stably at high temperatures (chemical formula is Y3A15O 12 ), belongs to the cubic system, has a garnet structure, Al 3+ and O 2- The vertices of the tetrahedron and octahedron formed are connected to form a three-dimensional skeleton structure. 3+ This special crystal structure gives YAG fiber excellent physical and chemical properties, with a melting point of 1942°C and a density of 4.55g / cm 3 , with isotropy, good chemical stability and good resistance to water vapor corrosion. YAG ceramics also have the advantages of high strength, small high-temperature creep and low thermal conductivity. These characteristics make it likely to become a new generation of high-temperature resistant structural materials.

[0003] YAG transparent ceramics can replace single crystal and glass laser materials and have broad application prospects. Whether it is used directly as a powder or made into a ceramic block, it is required to obtain powders with fine particles, high purity, uniform size distribution, no agglomeration, and a certain morphology. Therefore, YAG powder preparation technology has always been the focus of research by scholars at home and abroad. In addition, due to its excellent high-temperature performance, the fibers prepared with it can be used as reinforcements for metal or ceramic matrix composites and used in high-temperature oxidative environments such as aerospace.

[0004] Bruce H et al. of the University of Michigan prepared YAG fibers by the sol-gel method. Using a sol containing nano-scale Y2O3 and AlOOH colloidal particles as raw materials, polyethylene oxide was added as a colloidal stabilizer, and a spinning precursor with a certain viscosity was obtained after concentration, and YAG fibers were prepared by dry spinning (Journal of the American Ceramic Society, 1995, 78: 2141-2148). The fiber diameter is thick and the strength is low, so it is not suitable for weaving and is difficult to apply to ceramic-based composite materials. However, the bending stress relaxation test was used to evaluate its creep resistance at high temperatures, and it was found that it was superior to all commercial alumina fibers on the market, proving the excellent creep resistance of the YAG component. Li Chengshun et al. of Shandong University prepared YAG ceramic fibers by the sol-gel method. Aluminum powder and an aqueous solution of yttrium acetate (Y(OAc)3·4H2O) were used as raw materials, and ethylene oxide was added as a viscosity modifier to prepare a spinnable YAG sol (Materials Chemistry & Physics, 2009, 113: 31-35). Gel fibers with a diameter of 5-10 μm were prepared using centrifugal spinning technology, and YAG ceramic fibers were obtained by drying the gel fibers and heat treating them at a set temperature. However, the spinning raw materials prepared by this method contain Cl elements and spinning aids, which are not conducive to environmental protection and the preparation of high-performance fibers. In addition, since the spinning raw materials contain γ-AlOOH nanoparticles, phase separation is easily generated between the nanoparticles and the bulk oxide during the sintering process, which is not conducive to densification sintering. Sintering must be performed at a higher temperature, but high-temperature sintering will cause the grain size to increase, thereby affecting the mechanical properties of the fiber. Summary of the invention

[0005] The present invention provides a yttrium aluminum oxide ceramic precursor and a preparation method thereof. By introducing yttrium into a pure Al2O3 precursor system, a yttrium aluminum oxide continuous ceramic fiber having a YAG single crystal phase or an Al2O3-YAG complex phase is obtained. Taking advantage of the strong designability of the molecular components of the polymer precursor method, a YAG precursor and an Al2O3-YAG complex phase precursor with different composition ratios are designed and synthesized by adjusting the ratio of Y and Al elements, and a yttrium aluminum oxide continuous ceramic fiber is prepared through melt spinning and post-treatment processes.

[0006] The purpose of the present invention is to provide a yttrium aluminum oxide ceramic precursor and a preparation method thereof. Aluminum source and yttrium source are dissolved in an organic solvent according to a certain ratio, and the mixed solution is stabilized by coordination with a complexing agent and then hydrolyzed and polycondensed. According to different yttrium aluminum element ratios, the spinning performance of the precursor is improved by adjusting the synthesis process, and then yttrium aluminum oxide continuous ceramic fibers with different crystal phase compositions are prepared, and the high-temperature grain size stability and high-temperature resistance of the fiber are improved. The yttrium aluminum oxide ceramic precursor has a softening point between 110-180°C, and the ceramic yield is up to 39%.

[0007] The method for preparing a yttrium aluminum oxide ceramic precursor provided by the present invention comprises the following steps:

[0008] 1) Add aluminum source and yttrium source to the solvent, stir and reflux for 0.5-3h at a heating temperature of 60-110°C; add complexing agent at a heating temperature of 60-90°C, and reflux for 0.5-2h;

[0009] 2) adding a certain proportion of any one of the mixed solutions ac to the reaction system obtained in step 1), dropping at a certain speed, and reflux reacting for 1-3 hours after the dropping is completed; then performing reduced pressure or atmospheric distillation to remove the solvent and cool to room temperature to obtain a yttrium aluminum oxide ceramic precursor;

[0010] The mixed solution a is composed of water and ethylene glycol methyl ether;

[0011] The mixed solution b consists of water and ethylene glycol ether;

[0012] The mixed liquid c consists of water and n-propanol.

[0013] In step 1) of the above method, the aluminum source is selected from at least one of aluminum isopropoxide, aluminum n-propoxide and aluminum ethoxide;

[0014] The yttrium source is selected from at least one of yttrium acetylacetonate, yttrium isopropoxide, and yttrium acetate;

[0015] The amounts of the aluminum source and the yttrium source are converted into a molar ratio of Al to Y element of 5:3.5-0.5; specifically, it can be 5:3.5, 5:3, 5:2, 5:1, 5:0.5;

[0016] The solvent is selected from at least one of n-propanol, methanol and isopropanol;

[0017] The complexing agent is selected from at least one of diacetyl, acetylacetone and ethyl acetoacetate;

[0018] The molar amount of the complexing agent is 0.3-1 times the total molar amount of the aluminum source and the yttrium source;

[0019] In the step 2), the molar ratio of the total amount of the aluminum source and the yttrium source to water is 1:0.6-1; specifically 1:0.9;

[0020] In the mixed solution a, the mass ratio of water to ethylene glycol methyl ether is 1:1-10; specifically 1:6;

[0021] In the mixed solution b, the mass ratio of water to ethylene glycol ethyl ether is 1:1-10; specifically 1:2;

[0022] In the mixed solution c, the mass ratio of water to n-propanol is 1:1-10; specifically 1:4;

[0023] The dripping rate of any one of the mixed solutions ac is 0.5-5 drops / s; specifically 1 drop / s or 2 drops / s;

[0024] In the distillation step, the temperature is 180-270°C; specifically 260°C;

[0025] The distillation time is 0.5-6h; specifically 2h, 3.5h or 5h;

[0026] The softening point of the obtained yttrium aluminum oxide ceramic precursor is between 110-180°C.

[0027] In addition, the yttrium aluminum oxide ceramic precursor prepared according to the above method and the use of the yttrium aluminum oxide ceramic precursor in preparing fibers also fall within the protection scope of the present invention.

[0028] The fiber is prepared by melt spinning, and is a fiber containing aluminum and yttrium; specifically, it is a yttrium aluminum oxide continuous ceramic fiber having a YAG single crystal phase or an Al2O3-YAG complex phase.

[0029] In the above method, the molar ratio of Al to Y elements is 5:3, and atmospheric distillation is used, and the obtained fiber is single-phase YAG;

[0030] The molar ratio of Al to Y elements is greater than 5:3 (e.g., 5:3-0.5), and atmospheric distillation is used, and the crystal phase composition of the obtained fiber is YAG and Al2O3 phase;

[0031] The molar ratio of Al to Y is less than 5:3 (e.g., 5:3.5-3), and atmospheric distillation is used, and the crystal phase composition of the obtained fiber is YAG and YAM phases;

[0032] The molar ratio of Al to Y is 5:3 or less than 5:3 (e.g., 5:3.5-3), and vacuum distillation is used, and the fiber crystal phase composition of the obtained fiber is YAG and YAM phases;

[0033] The molar ratio of Al to Y elements is greater than 5:3 (such as 5:3-0.5) and vacuum distillation is used, and the crystal phase composition of the obtained fiber is YAG and Al2O3 phase.

[0034] The molar ratio of Al and Y elements and the distillation method (normal pressure or reduced pressure) will affect the fiber crystal phase composition. Reduced pressure distillation will cause partial loss of Al elements and thus affect the ratio of Al and Y elements.

[0035] The present invention has the following beneficial effects:

[0036] 1) The composition of the yttrium aluminum oxide ceramic precursor provided by the present invention is adjustable. By introducing yttrium element into the pure Al2O3 precursor system, yttrium aluminum oxide continuous ceramic fibers with a YAG single crystal phase or an Al2O3-YAG complex phase are obtained. Taking advantage of the strong designability of the molecular components of the polymer precursor method, by adjusting the ratio of Y and Al elements, YAG precursors and Al2O3-YAG complex phase precursors with different composition ratios are designed and synthesized, and yttrium aluminum oxide continuous ceramic fibers are prepared through melt spinning and post-treatment processes;

[0037] 2) The composition of the precursor is adjustable. By adjusting the synthesis process according to different yttrium-aluminum element ratios, the spinning performance of the precursor is improved, and yttrium aluminum oxide continuous ceramic fibers with different crystal phase compositions are prepared, thereby improving the high-temperature grain size stability and high-temperature resistance of the fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is a SEM image of the fiber in Example 1.

[0039] Figure 2 is the XRD pattern of the fiber prepared at different temperatures in Example 1.

[0040] Figure 3 This is the TG chart of the precursor in Example 1.

[0041] Figure 4 This is the SEM image of the fiber precursor in Example 2.

[0042] Figure 5 is the XRD pattern of the fiber prepared at different temperatures in Example 4. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0044] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0045] Example 1

[0046] Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 260°C for 4 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0047] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this example is 120° C., and the ceramic yield is 38.7%.

[0048] The yttrium aluminum oxide ceramic precursor was heated to 165°C, and after it was melted into a uniform melt and the residual bubbles were removed, it was melt-spun at a temperature of 165°C, with a filament hole diameter of 0.2mm, a screw extrusion force of 20MPa, and a spinning rate of 35Hz to obtain fiber precursors; the obtained fiber precursors were placed in a honeypot steam furnace, and water vapor was continuously introduced during the debinding and sintering process. The steam intake was 80L / h, and the temperature was raised to 6 at a heating rate of 0.5°C / min. The inorganic fiber was placed in an alumina fiber fast-sintering furnace with air as the atmosphere, and the temperature was raised to 1200°C at a rate of 10°C / min, kept at the target temperature of 600°C for 1 hour, and then cooled to room temperature to obtain an inorganic fiber. The inorganic fiber was placed in an alumina fiber fast-sintering furnace with air as the atmosphere, and the temperature was raised to 1200°C at a rate of 10°C / min. After being kept for 1 hour, the temperature was cooled to room temperature to obtain yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 1.56 GPa. The fiber crystal phase composition was YAG phase, and the average grain size was 23.4 nm.

[0049] The SEM image of the fiber is attached. Figure 1 .

[0050] The yttrium aluminum oxide ceramic precursor was ground into powder, and then excess water was added to react and then debinding was performed. The temperature was raised from room temperature to 700°C at a rate of 1°C / min and kept for 1 hour. The corresponding inorganic powder was obtained after the temperature was lowered to room temperature. The in-situ XRD pattern of the inorganic powder prepared from the precursor is shown in the attached figure. Figure 2. As can be seen from the figure, when the temperature rises to 900°C, the YAG fiber is basically amorphous, but there is a diffraction peak near 2θ=33°. Compared with the standard diffraction card of YAG (PDF#72-1315), it can be seen that the diffraction peak here is the characteristic peak of YAG, indicating that a small amount of YAG crystal phase has begun to form at 900°C. With the increase of temperature, the intensity of the YAG characteristic peak gradually increases and the peak width narrows, indicating that the grain size of the YAG fiber gradually increases and the lattice structure gradually completes. During the heating process, there is no intermediate phase YAP (YAlO3) and YAM (Y4Al2O9) in the crystal phase of the YAG fiber, indicating that a single-phase YAG fiber can be prepared by the polymer precursor method.

[0051] The TGA curve of the precursor in air atmosphere is attached. Figure 3 As can be seen from the figure, the weight loss of the YAG precursor from room temperature to 1350℃ can be divided into four stages. The weight loss rate from room temperature to 600℃ is about 50.6%, and the weight loss in this stage is mainly caused by the decomposition and departure of organic groups in the YAG precursor; the weight loss rate from 600℃ to 1050℃ is about 1%, and the weight loss curve in this stage tends to be flat; the weight loss rate from 1050℃ to 1250℃ is about 9.7%, and the weight loss in this stage is mainly caused by the removal of residual carbon in the YAG precursor; the weight loss rate from 1250℃ to 1350℃ is 0%, and the weight loss curve in this stage is flat, indicating that at 600℃, the inorganic process of the precursor has been basically completed, but due to the high thermal decomposition temperature of yttrium acetylacetonate contained in the YAG precursor, some residual carbon is still not removed after 600℃, and the residual weight rate of the precursor at 1350℃ is 38.7%.

[0052] Example 2

[0053] Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:2, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 240°C for 4.5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0054] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120°C, and the ceramic yield is 37.6%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 1), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 0.98 GPa are obtained. The fiber crystal phase composition is YAG phase and α-Al2O3 phase, and the average grain size is 72.8 nm.

[0055] See the attached SEM image of the fiber precursor. Figure 4 .

[0056] Example 3

[0057] Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:1, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 230°C for 5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0058] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this example is 120° C., and the ceramic yield is 36.2%.

[0059] The yttrium aluminum oxide ceramic precursor is heated to 165°C, and after it is melted into a uniform melt and the residual bubbles are removed, melt spinning is carried out at a temperature of 165°C, the diameter of the filament outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the filament is collected at a rate of 35Hz to obtain fiber precursor; the obtained fiber precursor is placed in a constant temperature and humidity chamber, heated to 85°C, kept warm at a relative humidity of 80% for 60 minutes, and cooled to room temperature. Subsequently, the fibers after steam cross-linking treatment were placed in a debinding and sintering integrated furnace for debinding to prepare inorganic fibers, the temperature was raised to 600°C at 1°C / min, kept at the target temperature of 600°C for 1 hour, and then cooled to room temperature to obtain inorganic fibers; the obtained inorganic fibers were placed in an alumina fiber fast-sintering furnace with air atmosphere, the temperature was raised to 1200°C at 10°C / min, kept at room temperature for 1 hour, and then cooled to room temperature to obtain yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10μm and an average tensile strength of 1.16GPa. The fiber crystal phase composition is YAG phase and α-Al2O3 phase, and the average grain size is 66.2nm.

[0060] Example 4

[0061] Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al to Y elements of 5:0.5, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 230°C for 6 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0062] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120°C, and the ceramic yield is 34.5%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 3), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 1.35 GPa are obtained. The fiber crystal phase composition is γ-Al2O3 phase, and the average grain size is 5.2 nm.

[0063] The XRD patterns of fibers prepared at different temperatures are shown in the attached Figure 5 . As can be seen from the figure, at 950°C and below, the fiber crystal phase composition is amorphous. When the temperature rises to 1000°C, the γ-Al2O3 phase begins to appear. At 1150°C, several sharp diffraction peaks appear, which belong to the YAG phase and YAlO3 phase. When the temperature rises to 1250°C, the characteristic diffraction peaks of the γ-Al2O3 phase and the YAlO3 phase disappear, indicating that these two crystal phases appear as intermediate phases, and the characteristic peaks of the α-Al2O3 phase begin to appear. The final crystal phase composition of the fiber is the YAG phase and the α-Al2O3 phase. With the increase of temperature, the characteristic peaks of the two crystal phases gradually increase and the peak width narrows, indicating that the grain size of the two crystal phases gradually increases and the lattice structure gradually becomes complete.

[0064] Example 5

[0065] Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3.5, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 270°C for 3.5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0066] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120° C., and the ceramic yield is 39.4%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 1), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 1.3 GPa are obtained. The fiber crystal phase composition is YAG phase and YAM phase, and the average grain size is 43.1 nm.

[0067] Example 6

[0068] Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; and vacuum distillation is performed at a heating temperature of 230°C for 2 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0069] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120° C., and the ceramic yield is 39.1%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 1), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 1.40 GPa are obtained. The fiber crystal phase composition is YAG phase and YAM phase, and the average grain size is 34.7 nm.

[0070] Example 7

[0071] Aluminum n-propoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:2, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, diacetyl in an amount of 0.6 times the molar fraction of the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol in a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; and vacuum distillation is performed at a heating temperature of 210°C for 2 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0072] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120°C, and the ceramic yield is 38.1%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 1), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 0.90 GPa are obtained. The fiber crystal phase composition is YAG phase and α-Al2O3 phase, and the average grain size is 73.4 nm.

[0073] Example 8

[0074] Aluminum isopropoxide and yttrium acetate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:1, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; and vacuum distillation is performed at a heating temperature of 200°C for 2.5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0075] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120°C, and the ceramic yield is 36.7%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 3), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 1.07 GPa are obtained. The fiber crystal phase composition is YAG phase and α-Al2O3 phase, and the average grain size is 68.3 nm.

[0076] Example 9

[0077] Aluminum ethoxide and yttrium isopropoxide are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:0.5, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; and vacuum distillation is performed at a heating temperature of 180°C for 3 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0078] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120°C, and the ceramic yield is 35.7%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 3), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 1.30 GPa are obtained. The fiber crystal phase composition is YAG phase and α-Al2O3 phase, and the average grain size is 42.9 nm.

[0079] Example 10

[0080] Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3.5, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, ethyl acetylacetate in an amount of 0.6 times the molar fraction of the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol in a mass ratio of 1:4 (wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6) is dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; and reduced pressure distillation is performed at a heating temperature of 230°C for 1.5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.

[0081] The softening point of the yttrium aluminum oxide ceramic precursor obtained in this embodiment is 120° C., and the ceramic yield is 39.7%. By melt spinning, steam crosslinking and debinding treatment and ceramic sintering (same as in Example 1), yttrium aluminum oxide continuous ceramic fibers with an average diameter of 10 μm and an average tensile strength of 1.3 GPa are obtained. The fiber crystal phase composition is YAG phase and YAM phase, and the average grain size is 67.1 nm.

[0082] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, and without the need to carry out unnecessary experimental conditions, the present invention can be implemented in a wide range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principles of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departure from the disclosed scope in the application, and changes made with conventional techniques known in the art.

Claims

1. A method for preparing a yttrium aluminum oxide ceramic precursor, comprising the following steps: 1) Add aluminum source and yttrium source to the solvent, stir and reflux for 0.5-3h at a heating temperature of 60-110°C; add complexing agent at a heating temperature of 60-90°C, and reflux for 0.5-2h; 2) adding a certain proportion of any one of the mixed solutions ac to the reaction system obtained in step 1), dropping at a certain speed, and reflux reacting for 1-3 hours after the dropping is completed; then performing reduced pressure or atmospheric distillation to remove the solvent and cool to room temperature to obtain a yttrium aluminum oxide ceramic precursor; The mixed solution a is composed of water and ethylene glycol methyl ether; The mixed solution b consists of water and ethylene glycol ether; The mixed liquid c consists of water and n-propanol.

2. The method according to claim 1, characterized in that: In step 1), the aluminum source is selected from at least one of aluminum isopropoxide, aluminum n-propoxide and aluminum ethoxide; The yttrium source is selected from at least one of yttrium acetylacetonate, yttrium isopropoxide, and yttrium acetate; The amounts of the aluminum source and the yttrium source are converted into a molar ratio of Al to Y elements of 5:3.5-0.

5.

3. The method according to claim 1, characterized in that: In step 1), the solvent is selected from at least one of n-propanol, methanol and isopropanol; The complexing agent is selected from at least one of diacetyl, acetylacetone and ethyl acetoacetate; The molar amount of the complexing agent is 0.3-1 times the total molar amount of the aluminum source and the yttrium source.

4. The method according to claim 1, characterized in that: In the step 2), the molar ratio of the total amount of the aluminum source and the yttrium source to water is 1:0.6-1; In the mixed solution a, the mass ratio of water to ethylene glycol methyl ether is 1:1-10; In the mixed solution b, the mass ratio of water to ethylene glycol ether is 1:1-10; In the mixed solution c, the mass ratio of water to n-propanol is 1:1-10.

5. The method according to claim 1, characterized in that: The dripping rate of any one of the mixed solutions ac is 0.5-5 drops / s; The temperature of the reduced pressure or normal pressure distillation is 180-270° C., and the time is 0.5-6 h.

6. The method according to claim 1, characterized in that: The softening point of the obtained yttrium aluminum oxide ceramic precursor is between 110-180°C.

7. A yttrium aluminum oxide ceramic precursor obtained by the method according to any one of claims 1 to 6.

8. Use of the yttrium aluminum oxide ceramic precursor according to claim 7 in preparing fibers.

9. The use according to claim 8, characterized in that: The fiber is a yttrium aluminum oxide continuous ceramic fiber with a YAG single crystal phase or an Al2O3-YAG complex phase.

Citation Information

Patent Citations

  • Preparation method of polycrystalline Al2O3-Y3Al5O12 complex-phase fibers or pure YAG fibers

    CN105002601A

  • Al-Si complex phase oxide continuous ceramic fiber and preparation method thereof

    CN111733484A

  • Al-Zr copolymerized oxide ceramic precursor and preparation method thereof

    CN113968974A

  • Preparation method for yttrium aluminum garnet continuous fiber

    US20200071231A1

  • Fabrication of Y3Al5O12 fibers from water soluble polymers

    US5352642A

Cited By

  • Method for preparing alumina fiber by sol-gel-electrostatic spinning method

    CN122382740A

  • A method for preparing alumina fibers by sol-gel-electrospinning

    CN122382740B