Preparation method and application of aluminum-doped zinc oxide target material

Through the preparation method of aluminum-doped zinc oxide target, the problem of insufficient density in magnetron sputtering coating is solved, and the high-quality preparation of high-frequency radio signal piezoelectric film is achieved, and industrial production is improved feasibility.

CN118908717APending Publication Date: 2024-11-08PEAK RUI RONGZE (HANGZHOU) ENTERPRISE CONSULTING MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983816.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the magnetron sputtering coating process, existing zinc oxide ceramic targets have uneven grain distribution, insufficient density, excessive grain size and bubble defects, resulting in the inability to effectively prepare high-frequency radio signal piezoelectric films, and the film is easy to be Shedding or uneven surfaces limit the value of large-scale industrial production.

Method used

The preparation method of aluminum-doped zinc oxide target is adopted, and the high density aluminum-doped zinc oxide target is obtained through cold isostatic pressing and sintering technology, which is used to prepare high-quality piezoelectric films for magnetron sputtering coating. Steps It includes cold isostatic molding of aluminum-doped zinc oxide nano powder, sintering in thermally conductive sand, and degumming to improve the compactness and uniformity of the target material.

Benefits of technology

The aluminum-doped zinc oxide target produced can form a piezoelectric film with uniform surface and consistent thickness, avoiding cracking and mold release problems. It is suitable for the preparation of high-frequency radio signal piezoelectric films of wafers above 8 inches, improving the industry. Feasibility of production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908717A_ABST
    Figure CN118908717A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of an aluminum-doped zinc oxide target material, and the preparation method of the aluminum-doped zinc oxide target material comprises the following steps: (1) carrying out cold isostatic pressing molding on aluminum-doped zinc oxide nano powder to obtain a biscuit; and (2) embedding the biscuit into heat-conducting sand, and sintering at the temperature of 1520-1550 DEG C to obtain the aluminum-doped zinc oxide target material. The preparation method has the advantages that the target material obtained through the preparation method can be made into the zinc aluminum oxide doped piezoelectric film with the uniform surface and the thickness ranging from 400 nm to 1000 nm, the obtained piezoelectric film can form a consistent piezoelectric coating film on the surface of a wafer with the diameter larger than 8 inches, and cracking and demolding are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a photoelectric functional material, and in particular to a preparation method and application of an aluminum-doped zinc oxide target material. Background Art

[0002] In recent years, with the introduction and realization of the concepts of intelligence and informatization, more and more electronic devices have appeared in people's lives: display screens, various sensors, solar cells, etc., and these devices, especially solar cells, require TCO films (transparent conductive films) as electrode layers or conductive layers. Zinc oxide target (ZnO) is a material with good visible light transmittance, high infrared reflectivity, wide band gap, and excellent conductivity. It has the advantages of wide material sources, good doping, and low cost. It is widely used in the preparation of TCO films.

[0003] Currently, ceramic targets doped with zinc oxide as the base are mass-produced on the market. Due to differences in powder and sintering processes, ceramic targets have defects such as uneven grain distribution, insufficient density, excessive grain size, and the presence of many bubbles. As a result, it is impossible to deposit the piezoelectric film with a thickness of 400-800 nanometers required in the field of radio communications through magnetron sputtering, the most commonly used and most economical coating method. Or after reaching the required thickness, the film is easy to fall off or the surface is uneven, resulting in waste. Therefore, it has no value for large-scale industrial production of high-frequency wireless piezoelectric films. Summary of the invention

[0004] The present invention provides a method for preparing an industrial-grade-sized zinc oxide aluminum-doped ceramic target material for processing high-quality, high-frequency radio signal piezoelectric films (covering the 5G wireless communication application frequency band) by magnetron sputtering coating and its application.

[0005] A first aspect of the present invention provides a method for preparing an aluminum-doped zinc oxide target, comprising the following steps:

[0006] (1) forming aluminum-doped zinc oxide nanopowder by cold isostatic pressing to obtain a green blank;

[0007] (2) The green blank is buried in thermal conductive sand and sintered at a temperature of 1520-1550° C. to obtain an aluminum-doped zinc oxide target.

[0008] According to some embodiments of the preparation method of the present invention, the pressure of the cold isostatic pressing is 225-250 MPa, preferably 250 MPa; for example, 225 MPa, 230 MPa, 235 MPa, 245 MPa, 250 MPa.

[0009] The cold isostatic pressing molding time is 10-20 minutes, such as 10 minutes, 15 minutes, 18 minutes, and 20 minutes. The best time for pressing molding is 15 minutes. If it is less than 15 minutes, the density of the green billet will decrease slightly. If it exceeds 15 minutes, the density will no longer increase. Therefore, 15 minutes is selected as the optimal holding time.

[0010] According to some embodiments of the preparation method of the present invention, the shape of the blank is a cuboid, the lengths of the long side and the short side of the blank are both 350-400 mm, and the thickness of the blank is 35-40 mm. The obtained blank can be used to make a 10-inch (about 254 mm) diameter ceramic rotary target, and the density of the blank is 95%-96%. The density after cold isostatic pressing is about 95%, and after sintering is greater than 95% and close to 96%.

[0011] According to some embodiments of the preparation method of the present invention, step (2) further includes a step of degumming the green blank.

[0012] According to some embodiments of the preparation method of the present invention, the degumming treatment method is heating the green blank.

[0013] According to some embodiments of the preparation method of the present invention, the heating temperature is 400-450° C., and the heating time is 3-4 days; further preferably, the heating is carried out in a degumming furnace.

[0014] According to some embodiments of the preparation method of the present invention, the thermal conductive sand is silicon dioxide quartz sand.

[0015] According to some embodiments of the preparation method of the present invention, the thickness of the thermal conductive sand coated green blank is 4-6 mm, for example, 4 mm, 5 mm, or 6 mm.

[0016] According to some embodiments of the preparation method of the present invention, the sintering time is 5-7 days; for example, 5 days, 6 days, 7 days.

[0017] According to some embodiments of the preparation method of the present invention, the sintering is normal pressure sintering.

[0018] According to some embodiments of the preparation method of the present invention, in step (2), the diameter of the aluminum-doped zinc oxide target is 250-260 mm, for example, 250 mm, 255 mm, 258 mm, 260 mm; the thickness is 4-6 mm, for example, 4 mm, 5 mm, 6 mm; the diameter after machining and cutting is the size of the circular target after machining, which can be directly used for coating on the machine, and the density of the aluminum-doped zinc oxide target is 95%-96%.

[0019] According to some embodiments of the preparation method of the present invention, the preparation method of the aluminum-doped zinc oxide nanopowder comprises the following steps:

[0020] a. Mixing zinc oxide, aluminum oxide, a dispersant and a defoaming agent and grinding them to obtain a mixture;

[0021] b. Mixing the mixture obtained in step a with a binder to obtain a slurry;

[0022] c. Drying and granulating the slurry obtained in step b to obtain the aluminum-doped zinc oxide nanopowder.

[0023] According to some embodiments of the preparation method of the present invention, in step a, the particle size of the zinc oxide is 0.8-1.2 um, and the particle size of the aluminum oxide is 0.8-1.2 um;

[0024] According to some embodiments of the preparation method of the present invention, the dispersant is water and / or SD-03 dispersant.

[0025] According to some embodiments of the preparation method of the present invention, the water is deionized water.

[0026] According to some embodiments of the preparation method of the present invention, the defoaming agent is n-butanol.

[0027] According to some embodiments of the preparation method of the present invention, the binder is PVA glue. PVA glue is polyvinyl alcohol glue, which is a water-soluble high molecular polymer widely used in many industries.

[0028] According to some embodiments of the preparation method of the present invention, the weight ratio of the zinc oxide to the aluminum oxide is (95-99.5):(5-0.5).

[0029] According to some embodiments of the preparation method of the present invention, the weight ratio of the dispersant, the defoaming agent and the aluminum oxide is 0.375:0.02:1.

[0030] According to some embodiments of the preparation method of the present invention, the grinding medium used in the grinding is zirconium oxide.

[0031] According to some embodiments of the preparation method of the present invention, the particle size of the zirconium oxide is 2-3 mm, preferably 3 mm.

[0032] According to some embodiments of the preparation method of the present invention, the grinding rotation speed is 30-50 r / min; for example, 30 r / min, 35 r / min, 38 r / min, 40 r / min, 43 r / min, 50 r / min.

[0033] According to some embodiments of the preparation method of the present invention, the grinding time is 20-28 hours; for example, 20 hours, 23 hours, 25 hours, 28 hours.

[0034] According to some embodiments of the preparation method of the present invention, the pH of the slurry is 8-9.5.

[0035] According to some embodiments of the preparation method of the present invention, in step c, the drying is centrifugal spray drying.

[0036] According to some embodiments of the preparation method of the present invention, the inlet air temperature of the centrifugal spray drying is 150-300°C, for example, 150°C, 180°C, 200°C, 230°C, 260°C, 280°C, 300°C.

[0037] According to some embodiments of the preparation method of the present invention, the atomization frequency of the centrifugal spray drying is 250-350 Hz, for example, 250 Hz, 280 Hz, 300 Hz, 320 Hz, 350 Hz.

[0038] The second aspect of the present invention provides an application of the aluminum-doped zinc oxide target obtained by the preparation method described in the first aspect of the present invention in the preparation of a piezoelectric film.

[0039] According to some embodiments of the application of the present invention, the piezoelectric film is a zinc oxide aluminum doped piezoelectric film of 400-1000nm; for example, 400nm, 500nm, 600nm, 700nm, 800nm, 1000nm.

[0040] The beneficial effects of the present invention are as follows: the target material obtained by the preparation method of the present invention can be made into a zinc oxide aluminum doped piezoelectric film with a uniform surface and a thickness of 400nm-1000nm. The obtained piezoelectric film can form a consistent piezoelectric coating on the surface of a wafer with a diameter of more than 8 inches without cracking or demolding. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a structural diagram of the aluminum-doped zinc oxide target prepared in Example 1 of the present invention;

[0042] Figure 2 This is a SEM image of the aluminum-doped zinc oxide target prepared in Example 1 of the present invention;

[0043] Figure 3 This is a structural diagram of the aluminum-doped zinc oxide target prepared in Comparative Example 1;

[0044] Figure 4 This is a structural diagram of the aluminum-doped zinc oxide target prepared in Comparative Example 2;

[0045] Figure 5This is the SEM image of the aluminum-doped zinc oxide target prepared in Comparative Example 3. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present disclosure. Such structures and technologies are also described in many publications.

[0047] Example 1

[0048] A method for preparing an aluminum-doped zinc oxide target comprises the following steps:

[0049] (1) 19.6 kg of zinc oxide (the particle size of zinc oxide is 1 um), 0.4 kg of aluminum oxide (the particle size of aluminum oxide is 1 um), 150 g of SD-03 dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0050] (2) mixing the ground mixture with 1800 g of PVA glue as a binder to obtain a slurry with a pH of 8;

[0051] (3) subjecting the slurry obtained in step (2) to centrifugal spray drying, wherein the air inlet temperature of the centrifugal spray drying is 260° C. and the atomization frequency of the centrifugal spray drying is 250 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained;

[0052] (4) The aluminum-doped zinc oxide nanopowder was pressed by cold isostatic pressing at a pressure of 225 MPa for 15 min to obtain a rectangular blank having a length and width of 350 mm, a thickness of about 40 mm, and a density of 95.07%;

[0053] (5) The green blank is placed in a degumming furnace and heated at 450°C for 3 days and then naturally cooled to room temperature. The green blank is then buried in thermal conductive sand (silicon dioxide quartz sand) so that the thickness of the thermal conductive sand covering the green blank is about 5 mm, and sintered at 1550°C for 6 days under normal pressure to obtain an aluminum-doped zinc oxide target; the target has a diameter of 250 mm and a thickness of 4 mm.

[0054] Example 2

[0055] A method for preparing an aluminum-doped zinc oxide target comprises the following steps:

[0056] (1) 19.6 kg of zinc oxide (the particle size of zinc oxide is 1 um), 0.4 kg of aluminum oxide (the particle size of aluminum oxide is 1 um), 150 g of SD-03 dispersant and 8.5 g of defoaming agent n-butanol are ground together, the grinding medium used is zirconium oxide with a particle size of 3 mm, the grinding speed is 30 r / min, and the grinding is performed for 20 hours to obtain a mixture;

[0057] (2) mixing the ground mixture with 1800 g of PVA glue as a binder to obtain a slurry with a pH of 8;

[0058] (3) subjecting the slurry obtained in step (2) to centrifugal spray drying, wherein the air inlet temperature of the centrifugal spray drying is 260° C. and the atomization frequency of the centrifugal spray drying is 250 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained;

[0059] (4) The aluminum-doped zinc oxide nanopowder was pressed by cold isostatic pressing at a pressure of 250 MPa for 15 min to obtain a rectangular blank having a length and width of 350 mm, a thickness of about 40 mm, and a density of 95.07%.

[0060] (5) The green blank is placed in a degumming furnace and heated at 400°C for 3 days and then naturally cooled to room temperature. The green blank is then buried in thermal conductive sand (silicon dioxide quartz sand) so that the thickness of the thermal conductive sand covering the green blank is about 5 mm, and sintered at 1520°C for 6 days under normal pressure to obtain an aluminum-doped zinc oxide target; the target has a diameter of 250 mm and a thickness of 5 mm.

[0061] Comparative Example 1

[0062] The only difference between Comparative Example 1 and Example 1 is that the green blank is not buried in the heat-conducting sand but is directly sintered.

[0063] Specifically:

[0064] (1) 19.6 kg of zinc oxide (the particle size of zinc oxide is 1 um), 0.4 kg of aluminum oxide (the particle size of aluminum oxide is 1 um), 150 g of SD-03 dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0065] (2) mixing the ground mixture with 1800 g of PVA glue as a binder to obtain a slurry with a pH of 8;

[0066] (3) subjecting the slurry obtained in step (2) to centrifugal spray drying, wherein the air inlet temperature of the centrifugal spray drying is 260° C. and the atomization frequency of the centrifugal spray drying is 250 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained;

[0067] (4) The aluminum-doped zinc oxide nanopowder was pressed by cold isostatic pressing at a pressure of 225 MPa for 15 min to obtain a rectangular blank having a length and width of 350 mm, a thickness of about 40 mm, and a density of 95.07%;

[0068] (5) The target blank is placed in a degumming furnace and heated at 450°C for 3 days and then naturally cooled to room temperature. It is then sintered at 1550°C for 6 days. After sintering, the target material cracks on a large scale and the target blank is scrapped and cannot be used.

[0069] Comparative Example 2

[0070] The difference between Comparative Example 2 and Example 1 is that only the bottom and side surfaces of the blank are covered.

[0071] Specifically:

[0072] (1) 19.6 kg of zinc oxide (the particle size of zinc oxide is 1 um), 0.4 kg of aluminum oxide (the particle size of aluminum oxide is 1 um), 150 g of SD-03 dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0073] (2) mixing the ground mixture with 1800 g of PVA glue as a binder to obtain a slurry with a pH of 8;

[0074] (3) subjecting the slurry obtained in step (2) to centrifugal spray drying, wherein the air inlet temperature of the centrifugal spray drying is 260° C. and the atomization frequency of the centrifugal spray drying is 250 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained;

[0075] (4) The aluminum-doped zinc oxide nanopowder was pressed by cold isostatic pressing at a pressure of 225 MPa for 15 min to obtain a rectangular blank having a length and width of 350 mm, a thickness of about 40 mm, and a density of 95.07%;

[0076] (5) The green blank was placed in a degumming furnace and heated at 450°C for 3 days and then naturally cooled to room temperature. The bottom and side surfaces of the green blank were then buried in thermal conductive sand (silicon dioxide quartz sand) so that the thickness of the thermal conductive sand covering the green blank was about 5 mm, and sintered at 1550°C for 6 days to obtain an aluminum-doped zinc oxide target. The edges of the prepared aluminum-doped zinc oxide target had a large number of small cracks, and could not be made into a large-size sputtering target.

[0077] Comparative Example 3

[0078] The difference between Comparative Example 3 and Example 1 is that the sintering temperature of the green billet is 1500° C. and the sintering time is 5.5 days.

[0079] Specifically:

[0080] (1) 19.6 kg of zinc oxide (the particle size of zinc oxide is 1 um), 0.4 kg of aluminum oxide (the particle size of aluminum oxide is 1 um), 150 g of SD-03 dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0081] (2) mixing the ground mixture with 1800 g of PVA glue as a binder to obtain a slurry with a pH of 8;

[0082] (3) subjecting the slurry obtained in step (2) to centrifugal spray drying, wherein the air inlet temperature of the centrifugal spray drying is 260° C. and the atomization frequency of the centrifugal spray drying is 250 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained;

[0083] (4) The aluminum-doped zinc oxide nanopowder was pressed by cold isostatic pressing at a pressure of 225 MPa for 15 min to obtain a rectangular blank having a length and width of 350 mm, a thickness of about 40 mm, and a density of 95.07%;

[0084] (5) The green blank was placed in a degumming furnace and heated at 450°C for 3 days and then naturally cooled to room temperature. The green blank was then buried in thermal conductive sand (silicon dioxide quartz sand) so that the thickness of the thermal conductive sand covering the green blank was about 5 mm, and sintered at 1500°C for 5.5 days to obtain an aluminum-doped zinc oxide target.

[0085] The SEM image of the aluminum-doped zinc oxide target prepared in Comparative Example 3 is as follows: Figure 5 As shown. Figure 1 and Figure 5 From the comparison, it can be seen that the aluminum-doped zinc oxide target prepared in Example 1 of the present invention is denser, has clearer lattice boundaries, more uniform lattice size distribution and fewer pores.

[0086] Comparative Example 4

[0087] The difference between Comparative Example 4 and Example 1 is that the cold pressing pressure of Comparative Example 4 is 200 MPa.

[0088] Specifically:

[0089] (1) 19.6 kg of zinc oxide (the particle size of zinc oxide is 1 um), 0.4 kg of aluminum oxide (the particle size of aluminum oxide is 1 um), 150 g of SD-03 dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0090] (2) mixing the ground mixture with 1800 g of PVA glue as a binder to obtain a slurry with a pH of 8;

[0091] (3) subjecting the slurry obtained in step (2) to centrifugal spray drying, wherein the air inlet temperature of the centrifugal spray drying is 260° C. and the atomization frequency of the centrifugal spray drying is 250 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained;

[0092] (4) The aluminum-doped zinc oxide nanopowder is pressed by cold isostatic pressing at a pressure of 200 MPa for 15 min to obtain a green blank with a rectangular structure;

[0093] (5) The green blank was placed in a degumming furnace and heated at 450°C for 3 days and then naturally cooled to room temperature. The green blank was then buried in thermal conductive sand (silicon dioxide quartz sand) so that the thickness of the thermal conductive sand covering the green blank was about 5 mm, and sintered at 1550°C for 6 days to obtain an aluminum-doped zinc oxide target.

[0094] The densities of the aluminum-doped zinc oxide target prepared in Comparative Example 4 and the aluminum-doped zinc oxide target prepared in Example 1 are shown in Table 1:

[0095] Table 1

[0096]

[0097]

[0098] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing an aluminum-doped zinc oxide target, characterized in that: The following steps are involved: (1) forming aluminum-doped zinc oxide nanopowder by cold isostatic pressing to obtain a green blank; (2) The green blank is buried in thermal conductive sand and sintered at a temperature of 1520-1550° C. to obtain an aluminum-doped zinc oxide target.

2. The preparation method according to claim 1, characterized in that: The cold isostatic pressing pressure is 225-250 MPa, preferably 250 MPa; The cold isostatic pressing molding time is 10-20 minutes.

3. The preparation method according to claim 1 or 2, characterized in that: The shape of the blank is a cuboid, the lengths of the long side and the short side of the blank are both 350-400 mm, the thickness of the blank is 35-40 mm, and the density of the blank is 95%-96%.

4. The preparation method according to claim 1 or 2, characterized in that: Step (2) further includes a step of degumming the green blank; preferably, the degumming method is heating the green blank; more preferably, the heating temperature is 400-450° C., and the heating time is 3-4 days; further preferably, the heating is carried out in a degumming furnace; The thermal conductive sand is silicon dioxide quartz sand; And / or, the thickness of the heat-conducting sand-coated green blank is 4-6 mm; And / or, the sintering time is 5-7 days; And / or, the sintering is normal pressure sintering.

5. The preparation method according to claim 4, characterized in that: In step (2), the diameter of the aluminum-doped zinc oxide target is 250-260 mm, the thickness is 4-6 mm, and the density of the aluminum-doped zinc oxide target is 95%-96%.

6. The preparation method according to claim 1, characterized in that: The method for preparing the aluminum-doped zinc oxide nanopowder comprises the following steps: a. Mixing zinc oxide, aluminum oxide, a dispersant and a defoaming agent and grinding them to obtain a mixture; b. Mixing the mixture obtained in step a with a binder to obtain a slurry; c. Drying and granulating the slurry obtained in step b to obtain the aluminum-doped zinc oxide nanopowder.

7. The preparation method according to claim 6, characterized in that: In step a, the particle size of the zinc oxide is 0.8-1.2 um; the particle size of the aluminum oxide is 0.8-1.2 um; And / or, the dispersant is water and / or SD-03 dispersant; preferably, the water is deionized water; And / or, the defoaming agent is n-butanol; And / or, the adhesive is PVA glue; And / or, the weight ratio of the zinc oxide to the aluminum oxide is (95-99.5):(5-0.5); and / or, the weight ratio of the dispersant, the defoaming agent and the alumina is 0.375:0.02:1; Preferably, the grinding medium used in the grinding is zirconium oxide; Preferably, the particle size of the zirconium oxide is 2-3 mm, preferably 3 mm; Preferably, the grinding speed is 30-50r / min; Preferably, the grinding time is 20-28 hours.

8. The preparation method according to claim 6 or 7, characterized in that: The pH of the slurry is 8-9.

5.

9. The preparation method according to claim 6, characterized in that: In step c, the drying is centrifugal spray drying; Preferably, the inlet air temperature of the centrifugal spray drying is 150-300°C, preferably 260°C; Preferably, the atomization frequency of the centrifugal spray drying is 250-350 Hz.