Glazed tile with gorgeous metal three-dimensional texture and preparation process
By spraying high-content silicon and heavy metal salt A dry grout, phosphate ink and protective glaze, the problem of difficulty in achieving concave and convex three-dimensional and colorful metal texture of ceramic tiles is solved, and the three-dimensional touch and colorful color of ceramic tiles are realized The metal texture overcomes the lack of realistic life of single metallic colors and concave and convex effects in the prior art.
Patent Information
- Application Number
- CN202411018931.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-29
AI Technical Summary
It is difficult for the existing technology to achieve the concave and convex three-dimensional effect and colorful metal texture of ceramic tiles at the same time. The existing metal glaze color is single, and it is impossible to effectively imitate the randomly distributed metal texture of high-end natural stone.
A dry granular slurry sprayed with high content of silicon and heavy metal salts, combined with ink and protective glaze with phosphate and soluble trivalent iron salts, is used to generate multi-layered metallic luster through high-temperature oxidation and reaction, forming a colorful metal three-dimensional texture.
It realizes the three-dimensional touch and colorful metal texture of ceramic tiles, overcomes the lack of realistic single metallic color and concave convex effects in the existing technology, and provides a richer decorative effect.
Smart Images

Figure CN118908752A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic tiles, and in particular to a glazed tile with colorful metallic three-dimensional texture and a preparation process thereof. Background Art
[0002] In the industry, marble tiles are mainly imitated by scanning patterns of marble materials. The imitation degree of surface effects such as concave and convex surfaces, sandblasted surfaces, flamed surfaces and metal texture surfaces is low, and the fidelity of concave and convex effects is low. It is especially difficult to imitate the randomly distributed metal texture of some high-end natural stones after polishing.
[0003] The existing technology currently usually uses powder to press a flat body or a mold body. In order to reflect the concave and convex three-dimensional effect on the flat body, dry particles, positioning glue dry particles, etc. are usually used to form a subtle concave and convex effect, but it can usually only show a concave and convex three-dimensional effect without other metal texture three-dimensional superposition; and the metal texture tiles in the industry are currently achieved by conventional single metal glaze, the color expression of the single metal glaze is relatively single, and there is no colorful metal texture effect. Summary of the invention
[0004] The main purpose of the present invention is to propose a preparation process of glazed tiles with colorful metallic three-dimensional texture, so as to overcome the technical problem that glazed tiles in the prior art are difficult to simultaneously achieve concave-convex three-dimensional effect and colorful metallic texture surface decoration effect. The secondary purpose of the present invention is to propose a glazed tile, which is prepared by the above-mentioned preparation process of colorful metallic three-dimensional texture.
[0005] To achieve the above object, the present invention proposes a preparation process of a glazed tile with a colorful metallic three-dimensional texture, comprising the following preparation steps:
[0006] S1, obtaining a green body by pressing;
[0007] S2, spraying dry particle slurry A to obtain a dry particle slurry spraying area A, wherein the dry material composition of the dry particle slurry A, in terms of weight parts, includes: 50-60 parts of dry particles A and 1-3.5 parts of heavy metal salts, and the raw material composition of the dry particles A, in terms of weight parts, includes: 60-76 parts of quartz powder, 10-17 parts of wollastonite, 5-8 parts of calcined kaolin, 3-5 parts of limestone, 3-7 parts of alumina powder and 4-10 parts of zirconium silicate, and the above raw materials are melted at high temperature, cooled, crushed, and sieved to obtain dry particles A;
[0008] S3, applying ink B to obtain a functional ink layer, the raw material composition of ink B, in terms of weight parts, includes: 8-18 parts of phosphate, 1-5.5 parts of dispersant and 70-80 parts of solvent, the above raw materials are mixed evenly and adjusted to a pH of 6-7 to obtain ink B;
[0009] S4, spraying C protective glaze on the outermost layer, the raw material composition of C protective glaze, by weight, includes: 15-25 parts of soluble trivalent iron salt, 7-12 parts of potassium feldspar, 8-13 parts of sodium feldspar, 1-2 parts of calcined alumina powder, 7-10 parts of calcined kaolin, 10-17 parts of calcined talc powder, 4-8 parts of calcined zinc oxide, 5-8 parts of barium carbonate and 5-12 parts of quartz powder, ball milling the above raw materials, mixing and sieving to obtain C protective glaze;
[0010] S5. After firing, glazed tiles are obtained.
[0011] Specifically, the green body obtained by pressing can be a flat green body or a mold green body. Even if the present invention is applied to a flat green body, a three-dimensional tactile effect can be achieved.
[0012] Specifically, the soluble trivalent iron salt is one or more of ferric chloride, ferric sulfate, ferric bromide, ferric iodide or ferric nitrate, which are not exhaustive here. Those skilled in the art can test and select the soluble trivalent iron salt with the best effect by considering cost, metallic gloss effect and impurity generation.
[0013] Preferably, the preparation step also includes a polishing process. The metallic luster in this embodiment is easily polished away by the conventional polishing process to remove the surface decorative effect. Exemplarily, the polishing process can be performed by lightly sweeping and polishing with a 240-mesh grinding brush to avoid cutting away the metallic luster. Those skilled in the art should understand that a shallow polishing or soft polishing process suitable for the preparation process of the present invention can be obtained through limited experiments to avoid cutting away the metallic luster effect on the surface.
[0014] Preferably, after step S1, a surface decoration step is also included, in which a decorative pattern layer is obtained on the blank or the A dry slurry spraying area or the functional ink layer by a known printing method such as inkjet penetration process, inkjet printing, roller printing, screen printing, etc.
[0015] The present invention obtains the A dry particle slurry spraying area by spraying A dry particle slurry, and the A dry particle has a semi-emulsified effect, and the silicon content in the main raw material is high, and the high-temperature viscosity is large, and the spraying area forms a three-dimensional effect. Under slightly acidic conditions, the phosphate in the B ink reacts with the C protective glaze to generate iron phosphate phase separation, and different saturations of imitation silver metallic luster are formed according to the different contents of iron phosphate produced by the reaction; at the same time, the heavy metal salt in the A dry particle slurry forms a new metallic color under high-temperature oxidation conditions, and part of the color area overlaps and combines with the imitation silver metallic color to form a colorful metallic luster.
[0016] Preferably, the particle size distribution of the powder in the A dry granules is:
[0017] ≥20 mesh 63~70%,
[0018] 20 mesh-40 mesh (<20 mesh, ≥40 mesh) 15-20%,
[0019] 40 mesh-60 mesh (<40 mesh, ≥60 mesh) 15-20%.
[0020] Powders smaller than 60 mesh are not used because fine powder cannot effectively form a concave-convex three-dimensional effect after sintering. The composition of the A dry particle raw material is combined with this particle size distribution to form a more significant three-dimensional effect in the A dry particle slurry spraying area.
[0021] More preferably, in the sintering process, the maximum sintering temperature is 1170-1225°C.
[0022] With this maximum firing temperature range, dry particles A can be fired well in the system.
[0023] Preferably, the diameter of the spray hole for spraying the dry particle slurry A is 1.5 mm to 2.3 mm, and the raw material of the protective glaze C is ball-milled and sieved to a fineness of 0.5-1.0% on a 325-mesh sieve to obtain the protective glaze C. With this number of spray holes, the dry particles A can be prevented from blocking the nozzle when spraying the dry particle slurry A.
[0024] Preferably, the soluble ferric iron salt is composed of 5-10 parts of ferric chloride and 10-15 parts of ferric bromide in terms of mass fractions.
[0025] Preferably, the heavy metal element in the heavy metal salt is at least one of copper, zinc, iron, nickel, manganese and cobalt; the phosphate is at least one of sodium phosphate Na3PO4 and calcium phosphate Ca3(PO4)2.
[0026] Preferably, the composition of ink B also includes 2-10 parts of pH regulator and 0.5-1.5 parts of defoamer by weight. For demonstration but not limitation, the pH regulator is DeuAdd MA-95 water-based acid-base pH regulator; the dispersant is ammonium polyacrylate; the solvent is diethylene glycol butyl ether ether solvent; and the defoamer is a fatty acid polymer substance. Those skilled in the art can confirm other pH regulators, defoamers, dispersants, solvents, etc. that are applicable to the present invention through limited experiments, and other additives that do not affect the surface decoration effect of the present invention can also be included.
[0027] Preferably, the functional ink layer occupies 35-50% of the surface area of the blank, and the A dry slurry spraying area occupies 50-70% of the surface area of the blank. Further preferably, the functional ink layer and the A dry slurry spraying area do not completely overlap.
[0028] By controlling the area ratio of the functional ink layer and the A dry slurry spraying area, after the overall spraying of the C protective glaze, the overlapping part of the functional ink layer and the A dry slurry spraying area presents a colorful metallic luster decorative effect, and the non-overlapping part of the functional ink layer and the A dry slurry spraying area presents an imitation silver metallic luster.
[0029] Preferably, in step S2, the specific gravity of the dry granular slurry A is 1.55-1.65 g / ml, and the glazing amount is 500-650 g / m2;
[0030] In step S3, the grayscale value of ink B is 10-100%, and the ink volume of ink B is 150-200 g / m2;
[0031] In step S4, the glazing amount of C protective glaze is 600-800 g / m2, and the specific gravity is 1.55-1.60 g / ml.
[0032] By controlling the specific gravity and glaze amount of dry slurry A, the gray value and ink amount of ink B, and the glaze amount and specific gravity of protective glaze C, the reaction between the metal salt in dry slurry A and ink B and protective glaze C can be fully ensured. Grayscale uses black tones to represent objects, and each grayscale object has a brightness value from 0% (white) to 100% (black). Different printing grayscales are set to control the phosphate content in ink B. After fully reacting with protective glaze C to form iron phosphate, it can present different shades of metallic luster.
[0033] The present invention also provides a glazed tile, characterized in that it is prepared by the preparation process of the glazed tile with colorful metallic three-dimensional texture in any of the above schemes. It has all the corresponding beneficial effects of the above schemes, which will not be described one by one here.
[0034] Compared with the prior art, the present invention provides a preparation process for glazed tiles with colorful metallic three-dimensional texture, wherein a dry granular slurry A spraying area is obtained by spraying a dry granular slurry A with a high silicon content and containing some heavy metal salts, and a three-dimensional effect is formed in the spraying area, and under slightly acidic conditions, the B ink reacts with the C protective glaze to generate iron phosphate phase separation, and different saturations of imitation silver metallic luster are formed according to the different contents of iron phosphate produced by the reaction; at the same time, the heavy metal salts in the dry granular slurry A form new colors under high-temperature oxidation conditions, and some color areas overlap and combine with the imitation silver metallic luster to form a colorful metallic luster. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying any creative work.
[0036] Figure 1 It is a schematic diagram of the glaze effect of the glazed tile with colorful metallic three-dimensional texture in the present invention.
[0037] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0039] In view of the technical problem that the metal glaze in the prior art has a single color and cannot show a concave-convex three-dimensional effect, the present application provides a preparation process for a glazed tile with a colorful metallic three-dimensional texture, including the following preparation steps:
[0040] S1, obtaining a green body by pressing;
[0041] S2, spraying dry particle slurry A to obtain a dry particle slurry spraying area A, wherein the dry material composition of the dry particle slurry A, in terms of weight parts, includes: 50-60 parts of dry particles A and 1-3.5 parts of heavy metal salts, and the raw material composition of the dry particles A, in terms of weight parts, includes: 60-76 parts of quartz powder, 10-17 parts of wollastonite, 5-8 parts of calcined kaolin, 3-5 parts of limestone, 3-7 parts of alumina powder and 4-10 parts of zirconium silicate, and the above raw materials are melted at high temperature, cooled, crushed, and sieved to obtain dry particles A;
[0042] S3, applying ink B to obtain a functional ink layer, the raw material composition of ink B, in terms of weight parts, includes: 8-18 parts of phosphate, 1-5.5 parts of dispersant and 70-80 parts of solvent, the above raw materials are mixed evenly and adjusted to a pH of 6-7 to obtain ink B;
[0043] S4, spraying C protective glaze on the outermost layer, the raw material composition of C protective glaze, by weight, includes: 15-25 parts of soluble trivalent iron salt, 7-12 parts of potassium feldspar, 8-13 parts of sodium feldspar, 1-2 parts of calcined alumina powder, 7-10 parts of calcined kaolin, 10-17 parts of calcined talc powder, 4-8 parts of calcined zinc oxide, 5-8 parts of barium carbonate and 5-12 parts of quartz powder, ball milling the above raw materials, mixing and sieving to obtain C protective glaze;
[0044] S5. After firing, glazed tiles are obtained.
[0045] In some specific embodiments, the pressed body is a flat body or a molded body, and the present application can achieve a three-dimensional tactile effect even when used on a flat body.
[0046] In some specific embodiments, the preparation steps also include a polishing process. The metallic luster in the present application is easily polished away by a conventional polishing process to remove the surface decorative effect. In a specific embodiment, the polishing process can be performed by lightly sweeping and polishing with a 240-mesh abrasive brush to avoid cutting away the metallic luster. Those skilled in the art should understand that a shallow polishing or soft polishing process suitable for the preparation process of the present invention can be obtained through limited experiments to avoid cutting away the metallic luster effect on the surface.
[0047] In some preferred embodiments, after step S1, a surface decoration step is also included, in which a decorative pattern layer is obtained on the blank or the A dry slurry spraying area or the functional ink layer by a known printing method such as inkjet penetration process, inkjet printing, roller printing, screen printing, etc.
[0048] In some specific embodiments, the slurry composition of dry particle slurry A includes, by weight percentage, 50-60 parts of dry particles A, 1-3.5 parts of heavy metal salt and 40-50 parts of suspension, and the suspension includes: 2.5-3.5 parts of sodium carboxymethyl cellulose and 100 parts of clean water, which are fully mixed and stirred, and the residue after passing through a 325-mesh sieve is 0%.
[0049] In some specific embodiments, the soluble ferric iron salt is composed of 5-10 parts of ferric chloride and 10-15 parts of ferric bromide, in parts by mass.
[0050] In some preferred embodiments, the particle size distribution of the powder in the A dry granules is:
[0051] ≥20 mesh 63~70%,
[0052] 20 mesh-40 mesh (<20 mesh, ≥40 mesh) 15-20%,
[0053] 40 mesh-60 mesh (<40 mesh, ≥60 mesh) 15-20%.
[0054] Powders with a sieve size smaller than 60 mesh are not used because fine powder cannot effectively form a concave-convex three-dimensional effect after sintering. The composition of dry granular raw materials A is matched with this particle size distribution to further improve the three-dimensional effect of the spraying area.
[0055] More preferably, in the sintering process, the maximum sintering temperature is 1170-1225°C.
[0056] In combination with this maximum firing temperature range, dry particles A can be fired well in the system.
[0057] More preferably, the diameter of the spray hole for spraying the dry particle slurry A is 1.5 mm-2.3 mm. With this mesh number of the spray hole, the situation in which the dry particles A block the nozzle can be prevented when spraying the dry particle slurry A.
[0058] In some preferred embodiments, the heavy metal element in the heavy metal salt is at least one of copper, zinc, iron, nickel, manganese and cobalt; the phosphate is at least one of sodium phosphate Na3PO4 and calcium phosphate Ca3(PO4)2.
[0059] In some preferred embodiments, the composition of ink B further includes 2-10 parts of a pH regulator and 0.5-1.5 parts of a defoaming agent by weight.
[0060] In some specific embodiments, the pH adjuster is DeuAdd MA-95 aqueous acid-base pH adjuster; the dispersant is ammonium polyacrylate; the solvent is diethylene glycol butyl ether solvent; and the defoamer is a fatty acid polymer substance.
[0061] In some preferred embodiments, the functional ink layer occupies 35-50% of the surface area of the blank, the A dry slurry spraying area occupies 50-70% of the surface area of the blank, and the functional ink layer and the A dry slurry spraying area do not completely overlap.
[0062] In some preferred embodiments, in step S2, the specific gravity of the dry granular slurry A is 1.55-1.65 g / ml, and the glazing amount is 500-650 g / m2;
[0063] In step S3, the grayscale value of ink B is 10-100%, and the ink volume of ink B is 150-200 g / m2;
[0064] In step S4, the glazing amount of C protective glaze is 600-800 g / m2, and the specific gravity is 1.55-1.60 g / ml.
[0065] The present application also proposes a glazed tile, which is prepared by the preparation process of the glazed tile with colorful metallic three-dimensional texture in any of the above-mentioned embodiments.
[0066] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0067] Example 1-1
[0068] Provided is a glazed tile, comprising the following preparation steps:
[0069] S1. The mold body is obtained by pressing. Here is a specific composition of the blank for example: the raw material composition of the blank includes, by mass, 12.5 parts of raw ore mud, 3.7 parts of bentonite, 9.6 parts of kaolin, 11.1 parts of washed mud, 29.5 parts of stone powder, 29.3 parts of potassium sand, 4 parts of talc and 0.3 parts of blank reinforcing agent. The above raw materials are ball-milled, mixed and sieved, and pressed to obtain the mold body.
[0070] S2, spraying A dry granular slurry to obtain A dry granular slurry spraying area,
[0071] In this embodiment, a slurry composition of A dry particle slurry is provided, which includes, by weight, 59.5 parts of A dry particles, 3.5 parts of heavy metal salts, and 38 parts of suspensions. The raw material composition of the suspension includes, by weight, 3 parts of sodium carboxymethyl cellulose and 100 parts of clean water. The suspension is prepared by uniformly mixing the raw materials and passing through a 325-mesh sieve with 0% residue.
[0072] The raw material composition of dry particles A, in parts by weight, includes: 66 parts of quartz powder, 13 parts of wollastonite, 6 parts of calcined kaolin, 4 parts of limestone, 5 parts of alumina powder and 6 parts of zirconium silicate. The above raw materials are melted at high temperature, cooled, crushed and sieved to obtain dry particles A.
[0073] The particle size distribution of the powder in dry granules A is: ≥20 mesh 39%, 20 mesh-40 mesh (<20 mesh, ≥40 mesh) 20%, 40 mesh-60 mesh (<40 mesh, ≥60 mesh) 23%, and <60 mesh 18%.
[0074] S3, applying ink B to obtain a functional ink layer. Specifically, in this embodiment, ink B and ordinary ink are used to obtain a decorative pattern layer combined with a functional ink layer by screen printing. In the embodiments or comparative examples, the ordinary inks mentioned are CIK-NE6118 ink produced by Foshan Yidajia Precision Ceramics Technology Co., Ltd., E3566 ink produced by Foshan Sanshui Kanglitai Inorganic Synthetic Materials Co., Ltd., and NGY-62016 and NGY-62012 inks produced by Foshan NGY Yangzi Pigment Co., Ltd.
[0075] The raw material composition of ink B includes, by weight: 18 parts of phosphate, 1 part of dispersant, 76 parts of solvent and 5 parts of pH adjuster. The above raw materials are mixed evenly and then adjusted to a pH of 6-7 to obtain ink B.
[0076] Among them, the heavy metal salt is cupric chloride, the phosphate is Na3PO4, the dispersant is ammonium polyacrylate, the solvent is diethylene glycol butyl ether, and the pH adjuster is DeuAdd MA-95 aqueous acid-base pH adjuster.
[0077] S4. Spray C protective glaze on the outermost layer. The raw materials of C protective glaze, calculated by weight, include: 15 parts of soluble iron salt, 12 parts of potassium feldspar, 13 parts of sodium feldspar, 1 part of calcined alumina powder, 10 parts of calcined kaolin, 17 parts of burned talc powder, 8 parts of calcined zinc oxide, 5 parts of barium carbonate and 12 parts of quartz powder. The above raw materials are ball-milled, mixed and sieved to obtain C protective glaze.
[0078] The soluble iron salt is composed of 15 parts of ferric chloride, and the raw materials of C protective glaze are ball-milled and sieved to a fineness of 0.5% on a 325-mesh sieve to obtain C protective glaze.
[0079] S5. After firing, glazed tiles are obtained.
[0080] Among them, in the firing process, the highest firing temperature is 1170°C.
[0081] In this embodiment, the functional ink layer occupies 40% of the surface area of the blank, the A dry slurry spraying area occupies 40% of the surface area of the blank, and the functional ink layer and the A dry slurry spraying area completely overlap.
[0082] In step S2, the specific gravity of dry slurry A is 1.40 g / ml, and the glazing amount is 450 g / m2; in step S3, the grayscale value of ink B is 10-100%, and the ink amount of ink B is 100 g / m2; in step S4, the glazing amount of protective glaze C is 500 g / m2, and the specific gravity is 1.50 g / ml.
[0083] Example 1-2
[0084] Provided is a glazed tile, comprising the following preparation steps:
[0085] S1, obtaining a planar green body by pressing;
[0086] The specific raw material composition of the blank in Example 1-1 is adopted; the above raw materials are ball-milled, mixed, sieved, and pressed to obtain a flat blank.
[0087] S2. Spray dry particle slurry A to obtain a dry particle slurry spraying area A. In this embodiment, a slurry composition of dry particle slurry A is provided, which includes, by weight, 50 parts of dry particles A, 1 part of heavy metal salt and 49 parts of suspension. The raw material composition and preparation method of the suspension refer to Example 1-1.
[0088] The raw material composition of dry particles A, in parts by weight, includes: 60 parts of quartz powder, 17 parts of wollastonite, 5 parts of calcined kaolin, 5 parts of limestone, 3 parts of alumina powder and 10 parts of zirconium silicate. The above raw materials are melted at high temperature, cooled, crushed and sieved to obtain dry particles A.
[0089] The particle size distribution of the powder in dry granules A is: ≥20 mesh 70%, 20 mesh-40 mesh (<20 mesh, ≥40 mesh) 15%, 40 mesh-60 mesh (<40 mesh, ≥60 mesh) 15%.
[0090] S3. Apply ink B to obtain a functional ink layer. Specifically, in this embodiment, ink B and ordinary ink are loaded into different channels, and are sprayed by inkjet printing to obtain a decorative pattern layer combined with the functional ink layer.
[0091] The raw material composition of ink B includes, by weight: 8 parts of phosphate, 5.5 parts of dispersant, 1.5 parts of defoamer, 80 parts of solvent and 5 parts of pH adjuster. The above raw materials are mixed evenly and the pH is adjusted to 6-7 to obtain ink B.
[0092] Among them, the heavy metal salts are nickel sulfate and manganese sulfate, the phosphate is Na3PO4 and Ca3(PO4)2 in a 1:1 (weight ratio), the dispersant is ammonium polyacrylate, the solvent is diethylene glycol butyl ether, and the pH adjuster is DeuAdd MA-95 aqueous acid-base pH adjuster.
[0093] S4. Spray C protective glaze on the outermost layer. The raw materials of C protective glaze, calculated by weight, include: 25 parts of soluble iron salt, 8 parts of potassium feldspar, 13 parts of sodium feldspar, 2 parts of calcined alumina powder, 10 parts of calcined kaolin, 17 parts of burned talc powder, 8 parts of calcined zinc oxide, 7 parts of barium carbonate and 10 parts of quartz powder. The above raw materials are ball-milled, mixed and sieved to obtain C protective glaze.
[0094] The soluble iron salt is composed of 15 parts of ferric chloride and 10 parts of ferric bromide. The raw materials of C protective glaze are ball-milled and sieved to a fineness of 0.5% on a 325-mesh sieve to obtain C protective glaze.
[0095] S5. After firing and polishing steps, glazed tiles are obtained.
[0096] Among them, in the firing process, the highest firing temperature is 1200°C, and the polishing process is to use a 240-mesh grinding brush for light brushing.
[0097] In this embodiment, the functional ink layer occupies 50% of the surface area of the blank, the A dry slurry spraying area occupies 50% of the surface area of the blank, and the functional ink layer and the A dry slurry spraying area do not completely overlap.
[0098] In step S2, the specific gravity of dry slurry A is 1.55 g / ml, and the glazing amount is 500 g / m2; in step S3, the grayscale value of ink B is 10-100%, and the ink amount of ink B is 150 g / m2; in step S4, the glazing amount of protective glaze C is 600 g / m2, and the specific gravity is 1.55 g / ml.
[0099] Examples 1-3
[0100] Provided is a glazed tile, comprising the following preparation steps:
[0101] S1, obtaining a planar green body by pressing;
[0102] The specific raw material composition of the blank in Example 1-1 is adopted; the above raw materials are ball-milled, mixed, sieved, and pressed to obtain a flat blank.
[0103] S2, spraying A dry granular slurry to obtain A dry granular slurry spraying area,
[0104] In this embodiment, a slurry composition of A dry particles is provided, which includes, by weight, 51.5 parts of A dry particles, 3.5 parts of heavy metal salts and 45 parts of suspension. The raw material composition and preparation method of the suspension refer to Example 1-1.
[0105] The raw material composition of dry particles A, in parts by weight, includes: 70 parts of quartz powder, 10 parts of wollastonite, 7 parts of calcined kaolin, 3 parts of limestone, 6 parts of alumina powder and 4 parts of zirconium silicate. The above raw materials are melted at high temperature, cooled, crushed and sieved to obtain dry particles A.
[0106] The particle size distribution of the powder in dry granules A is: ≥20 mesh 63%, 20 mesh-40 mesh (<20 mesh, ≥40 mesh) 17%, 40 mesh-60 mesh (<40 mesh, ≥60 mesh) 20%.
[0107] S3. Apply ink B to obtain a functional ink layer. Specifically, in this embodiment, ink B and ordinary ink are loaded into different channels, and are sprayed by inkjet printing to obtain a decorative pattern layer combined with the functional ink layer.
[0108] The raw material composition of ink B includes, by weight, 15 parts of phosphate, 4.5 parts of dispersant, 0.5 parts of defoamer, 70 parts of solvent and 10 parts of pH adjuster.
[0109] The above raw materials were mixed evenly and the pH was adjusted to 6-7 to obtain ink B.
[0110] Among them, the heavy metal salts are nickel sulfate, manganese sulfate and cobalt chloride, the phosphate is Ca3(PO4)2, the dispersant is ammonium polyacrylate, the solvent is diethylene glycol butyl ether, and the pH adjuster is DeuAdd MA-95 aqueous acid-base pH adjuster.
[0111] S4. Spray C protective glaze on the outermost layer. The raw materials of C protective glaze, calculated by weight, include: 25 parts of soluble iron salt, 11 parts of potassium feldspar, 11 parts of sodium feldspar, 1.5 parts of calcined alumina powder, 8 parts of calcined kaolin, 16 parts of burned talc powder, 7.5 parts of calcined zinc oxide, 7 parts of barium carbonate and 6 parts of quartz powder. Ball-mill the above raw materials, mix and sieve to obtain C protective glaze.
[0112] The soluble iron salt is composed of 10 parts of ferric chloride and 15 parts of ferric bromide. The raw materials of C protective glaze are ball-milled and sieved to a fineness of 1.0% on a 325-mesh sieve to obtain C protective glaze.
[0113] S5. After firing and polishing steps, glazed tiles are obtained.
[0114] The highest firing temperature in the firing process is 1225° C. The polishing process is performed by lightly brushing with a 240-mesh abrasive brush.
[0115] In this embodiment, the functional ink layer occupies 35% of the surface area of the blank, the A dry slurry spraying area occupies 70% of the surface area of the blank, and the functional ink layer and the A dry slurry spraying area do not completely overlap.
[0116] In step S2, the specific gravity of dry slurry A is 1.65 g / ml, and the glazing amount is 650 g / m2; in step S3, the grayscale value of ink B is 10-100%, and the ink amount of ink B is 200 g / m2; in step S4, the glazing amount of protective glaze C is 800 g / m2, and the specific gravity is 1.60 g / ml.
[0117] The overlapping areas of the glazed tiles prepared in the above embodiment were randomly sampled to test the color development, glossiness and concave-convex height. The effect data are as follows:
[0118]
[0119]
[0120] Note: In the glazed tiles, the C protective glaze is on the outermost layer. The ABC overlapping area refers to the area where the functional ink layer overlaps with the A dry slurry spraying area. The AC overlapping area refers to the area where the A dry slurry spraying area does not overlap with the functional ink layer. The BC overlapping area refers to the area where the functional ink layer does not overlap with the A dry slurry spraying area. Three sampling areas with an area of 2mm*2mm are randomly selected in each overlapping area.
[0121] From the above data, it can be seen that in Example 1-1, since the particle size of dry granular powder A, the gray scale of ink B, the amount of ink, the amount of glaze applied by dry granular slurry A and protective glaze C and the specific gravity are not within the preferred range, the reaction is not sufficient, the color tone generated in the overlapping area of ABC is lighter, and its three-dimensional effect is average compared with that of Example 1-2 and Example 1-3. Moreover, since the functional ink layer completely overlaps with the spraying area of dry granular slurry A, it does not produce different decorative effects in the overlapping area of AC or BC as in Example 1-2 and Example 1-3. However, since Example 1-1 is within the preferred raw material composition ratio range of dry granular slurry A, ink B and protective glaze C in this scheme, colorful metallic luster is still formed in the overlapping area of ABC. Among them, Example 1-2 is the best embodiment, and its three-dimensional effect is the most prominent, and the colors are colorful, the tones are deep and elegant, the luster of the three different overlapping areas is layered and not abrupt, and the overall light feeling is the most comfortable.
[0122] Comparative Example 1
[0123] The difference from Example 1-2 is that after the flat body is pressed in step S1, conventional metal glaze is applied to the surface of the body. In this comparative example, DS08500 metal glaze produced by Guangdong Dow Technology Co., Ltd. is used, and the metal glazed tiles of the prior art are obtained by firing.
[0124] Comparative Example 2
[0125] The difference from Example 1-2 is that only ordinary ink is used in step S3. (The ink does not contain phosphoric acid)
[0126] Comparative Example 3
[0127] The difference from Example 1-2 is that the raw material composition of the dry particle slurry A in step S2 does not contain heavy metal salts.
[0128] The overlapping areas of the glazed tiles prepared in the above comparative example were randomly sampled to test the color development, glossiness and concave-convex height, and compared with Examples 1-2. The effect data are as follows:
[0129]
[0130]
[0131] By comparing the effect data of the conventional metallic glaze in comparative example 1 with those of embodiments 1-2, it can be seen that the metallic color of the conventional metallic glaze is single and has no three-dimensional effect; in comparative example 2, ordinary ink is used instead of ink B, which cannot react with dry particle slurry A or protective glaze C, and therefore no colorful metallic luster is formed, and the color in the randomly sampled area is single; in comparative example 3, no heavy metal salt is added to the raw material composition of dry particle slurry A, and the ceramic tiles obtained have only a single metallic luster generated by the reaction of the functional ink layer and the protective glaze C, and similarly, no colorful metallic luster effect can be formed.
[0132] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A process for preparing glazed tiles with colorful metallic three-dimensional texture, characterized in that: The method comprises the following preparation steps: S1, obtaining a green body by pressing; S2, spraying A dry particle slurry to obtain A dry particle slurry spraying area, wherein the dry material composition of the A dry particle slurry, by weight, includes: 50-60 parts of A dry particles and 1-3.5 parts of heavy metal salts, and the raw material composition of the A dry particles, by weight, includes: 60-76 parts of quartz powder, 10-17 parts of wollastonite, 5-8 parts of calcined kaolin, 3-5 parts of limestone, 3-7 parts of alumina powder and 4-10 parts of zirconium silicate, and the above raw materials are melted at high temperature, cooled, crushed, and sieved to obtain the A dry particles; S3, applying ink B to obtain a functional ink layer, wherein the raw material composition of ink B includes, by weight, 8-18 parts of phosphate, 1-5.5 parts of dispersant and 70-80 parts of solvent, and the above raw materials are mixed uniformly and adjusted to a pH of 6-7 to obtain ink B; S4, spraying C protective glaze on the outermost layer, wherein the raw material composition of the C protective glaze, by weight, includes: 15-25 parts of soluble trivalent iron salt, 7-12 parts of potassium feldspar, 8-13 parts of sodium feldspar, 1-2 parts of calcined alumina powder, 7-10 parts of calcined kaolin, 10-17 parts of calcined talc powder, 4-8 parts of calcined zinc oxide, 5-8 parts of barium carbonate and 5-12 parts of quartz powder, ball-milling the above raw materials, mixing and sieving to obtain the C protective glaze; S5. After firing, glazed tiles are obtained.
2. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: After step S1, a surface decoration step is also included, in which a decorative pattern layer is obtained on the blank or the A dry slurry spraying area or the functional ink layer by a known printing method.
3. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: The particle size distribution of the powder in the A dry granules is: ≥20 mesh 63~70%, 20 mesh-40 mesh (<20 mesh, ≥40 mesh) 15-20%, 40 mesh-60 mesh (<40 mesh, ≥60 mesh) 15-20%.
4. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: In the sintering process, the highest sintering temperature is 1170-1225°C.
5. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: The diameter of the spray hole for spraying the dry granular slurry A is 1.5 mm to 2.3 mm.
6. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: The heavy metal element in the heavy metal salt is at least one of copper, zinc, iron, nickel, manganese and cobalt; the phosphate is at least one of sodium phosphate Na3PO4 and calcium phosphate Ca3(PO4)2.
7. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: The composition of the ink B also includes 2 to 10 parts of a pH regulator and 0.5 to 1.5 parts of a defoamer by weight, wherein the pH regulator is DeuAdd MA-95 aqueous acid-base pH regulator; the dispersant is ammonium polyacrylate; the solvent is a diethylene glycol butyl ether solvent; and the defoamer is a fatty acid polymer substance.
8. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: The functional ink layer occupies 35-50% of the surface area of the blank, the A dry slurry spraying area occupies 50-70% of the surface area of the blank, and the functional ink layer does not completely overlap with the A dry slurry spraying area.
9. The process for preparing the glazed tile with colorful metallic three-dimensional texture according to claim 1, characterized in that: In step S2, the specific gravity of the A dry slurry is 1.55-1.65g / ml, and the glazing amount is 500-650g / m2; in step S3, the grayscale value of the B ink is 10-100%, and the ink amount of the B ink is 150-200g / m2; in step S4, the glazing amount of the C protective glaze is 600-800g / m2, and the specific gravity is 1.55-1.60g / ml.
10. A glazed tile, characterized in that: The glazed tile with colorful metallic three-dimensional texture is prepared by the preparation process of any one of claims 1 to 9.
Citation Information
Patent Citations
Geshi metal glaze with copper red metal texture and processing technology thereof
CN112811818A
Ceramic tile with starlight three-dimensional effect and preparation method thereof
CN114276121A
Preparation method of pearl dry particles, pearl glaze and pearl glazed tile
CN116023029A
Colorful marble tile with 3D digital mold effect and preparation method of colorful marble tile
CN118145975A
Large-particle ceramic glaze with a high content of solids
US20190292093A1