Preparation method of C9 cold polymerized resin with narrow molecular weight, high toughness and good processability

Through the process of distillation and compounding catalyst dropwise reaction, the problem of insufficient performance of traditional cold poly resins was solved, and C9 cold poly resin with narrow molecular weight, high toughness and good processing performance was prepared. It is suitable for the new energy field and meets the new Demand in the energy sector and reduce costs.

CN118909188APending Publication Date: 2024-11-08GUANGDONG NEWHUAYUE PETROCHEMICAL GROUP STOCK COMPANY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410976558.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional cold poly resins have shortcomings in terms of mechanical properties, stability and processing properties, and are difficult to meet the needs of the new energy field, especially their wide molecular weight, toughness and stability are not ideal.

Method used

Through distillation treatment and specific preparation processes, a dropwise reaction is performed using a compound catalyst and a cocatalyst, combined with an inert gas to warm up and polymerize, and the oligomer is removed through liquid alkali termination and reduced pressure distillation to prepare a narrow molecular weight and high toughness and C9 cold poly resin with good processing performance.

Benefits of technology

The narrow molecular weight of cold poly resin is achieved, and its toughness, stability and processing performance is improved. It is suitable for the manufacture of products in special environments such as solar panels, reducing costs and improving reaction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a C9 cold polymerized resin with narrow molecular weight, high toughness and good processability and a preparation method thereof, and aims to provide a cold polymerized resin with narrow molecular weight and high stability, the cold polymerized resin has excellent mechanical properties and stability, and the technical scheme of the cold polymerized resin sequentially comprises the following steps: step 1, carrying out rectification treatment on a C9 fraction, cutting light components and heavy components in the C9 fraction; step 2, adding the pretreated C9 into a reaction kettle, dropwise adding the compounded catalyst and the cocatalyst in a metering manner at the temperature of 5-15 DEG C, and continuously stirring for pre-reaction after dropwise adding is finished; 3, inert gas with the pressure of 0.1 Mpa to 0.5 Mpa is introduced, the temperature is increased to 30 DEG C to 40 DEG C, and a polymerization reaction is conducted for 3 h to 4 h; step 4, cooling to normal temperature after the reaction is finished, transferring the polymer liquid after the reaction to a neutralization kettle, adding pre-prepared liquid caustic soda, and terminating the polymerization reaction; washing with water to be neutral to obtain a polymerization reaction solution; and step 5, carrying out reduced pressure distillation on the polymerization reaction solution to remove oligomers so as to obtain the C9 cold polymerized resin with narrow molecular weight, high toughness and good processability. Belongs to the technical field of resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resins, in particular to a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance and a preparation method thereof. Background Art

[0002] Methylstyrene, dicyclopentadiene and indene are all important organic chemical raw materials with wide application value. However, the utilization of these raw materials is mainly concentrated in a single synthesis or processing process, and their synergistic effects and applications in cold polymerization reactions have not been fully studied.

[0003] As an important polymer material, cold-polymerized resin has a wide range of applications. However, traditional cold-polymerized resin has certain deficiencies in mechanical properties and stability, making it difficult to meet the needs of the new energy field.

[0004] CN202111636997.6 discloses a low softening point, high molecular weight C9 cold polymerization resin product and a preparation method thereof, comprising the following steps: Step 1, depolymerizing dicyclopentadiene in the C9 raw material into cyclopentadiene;

[0005] Step 2: distill the depolymerized raw material to remove light components and heavy components, and divide the depolymerized raw material into styrene fraction and indene fraction according to the boiling point of the intermediate component; Step 3: mix the styrene fraction, indene fraction, styrene, indene, and solvent oil to obtain the reaction raw material, and add the catalyst to carry out polymerization reaction; Step 4: after the reaction, wash with alkali and water respectively to obtain C9 cold polymerization resin polymerization liquid, and then remove the solvent, unreacted monomers and oligomers through distillation, stripping and other methods to obtain C9 cold polymerization resin. However, the catalyst used in this scheme is one or more of single catalyst aluminum trichloride, boron trifluoride ether complex, and boron trifluoride; although the product prepared by it has a low softening point and a high molecular weight, its molecular weight is wide, and its toughness, stability, and processing performance are still not ideal, which is difficult to meet the needs of special environments. Summary of the invention

[0006] In view of the above-mentioned shortcomings, the first object of the present invention is to provide a cold-polymerized resin with narrow molecular weight and high stability, which has excellent mechanical properties and stability and is suitable for the new energy field.

[0007] The second object of the present invention is to provide a method for preparing a cold-polymerized resin with a narrow molecular weight and high stability. The method achieves the narrow molecular weight, high toughness and good processing performance of the cold-polymerized resin through a specific preparation process and formula design.

[0008] To this end, the first technical solution provided by the present invention is:

[0009] A method for preparing a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance comprises the following steps in sequence:

[0010] Step 1, distilling the C9 fraction to cut the light components and heavy components in the C9 fraction;

[0011] Step 2: Add the pretreated C9 into the reactor, and add the compounded catalyst and co-catalyst dropwise in a metered manner at a temperature of 5-15°C, and continue stirring to perform a pre-reaction after the addition is completed;

[0012] Step 3: introduce 0.1Mpa-0.5Mpa inert gas, raise the temperature to 30°C-40°C and carry out polymerization reaction for 3h-4h;

[0013] Step 4: After the reaction is completed, the temperature is lowered to room temperature, and the polymer solution after the reaction is transferred to a neutralization kettle, and a pre-prepared liquid alkali is added to terminate the polymerization reaction; and then the polymer solution is washed with water until it is neutral to obtain a polymerization reaction solution;

[0014] Step 5, distilling the polymerization reaction liquid under reduced pressure to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance;

[0015] The total amount of the catalyst and the co-catalyst added is 0.5-1.5% of the mass of the reaction material;

[0016] The percentage of the promoter in the reaction material is 0.05-0.2%.

[0017] The reaction process is:

[0018]

[0019] Furthermore, in the above-mentioned method for preparing a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance, the dropping time in step 2 is 0.1h-1h.

[0020] Furthermore, in the above-mentioned method for preparing a C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance, the liquid alkali in step four is one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution, and ammonia solution, and the concentration of the liquid alkali is 30wt%.

[0021] Furthermore, in the above-mentioned method for preparing a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance, the temperature for removing oligomers by reduced pressure distillation in step 5 is 100°C-150°C, and the negative pressure condition is 700-1000 Pa.

[0022] Furthermore, the above-mentioned C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance, the C9 raw material contains methyl styrene, dicyclopentadiene and indene components.

[0023] Further, the above-mentioned narrow molecular weight, high toughness and good processing performance C9 cold polymerization resin, the catalyst is BF 3 Complex catalyst, AlCl 3 At least one of a catalyst, a boron trifluoride ether solution, and boron trifluoride.

[0024] Furthermore, in the above-mentioned C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance, the co-catalyst is at least one of triisobutylaluminum, molybdenum pentachloride and ethylaluminum dichloride.

[0025] Furthermore, the above-mentioned narrow molecular weight, high toughness and good processing performance C9 cold polymerization resin, the composite catalyst is BF 3 Complex catalysts and AlCl 3 Compounds:

[0026] Furthermore, in the above-mentioned C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance, the inert gas is nitrogen.

[0027] Furthermore, in the above-mentioned C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance, the C9 fraction is distilled in step 1 to collect light components with a distillation range of 120-200°C.

[0028] Furthermore, in the above-mentioned C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance, the supplementary component is methyl styrene or dicyclopentadiene or indene.

[0029] The C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance provided by the present invention is prepared by the method described in the first technical solution.

[0030] Compared with the prior art, the technical solution provided by the present invention has the following technical advantages:

[0031] 1. The cold-polymerized resin provided by the present invention achieves a narrow molecular weight of the cold-polymerized resin through reasonable formula design and preparation process, meets the needs of the new energy field, and can be used to manufacture solar cell panels (resin power cover panels).

[0032] 2. The cold-polymerized resin provided by the present invention has high toughness: The cold-polymerized resin provided by the present invention has good toughness and can adapt to relatively high-strength stretching.

[0033] 3. The cold-polymerized resin provided by the present invention has high stability: The cold-polymerized resin provided by the present invention has excellent stability and can maintain good performance under various environmental conditions.

[0034] 4. The cold-polymerized resin provided by the present invention has good processing properties: The cold-polymerized resin provided by the present invention has good processing properties and can be easily processed into products of various shapes and sizes.

[0035] 5. The cold-polymerized resin provided by the present invention has the advantages of improving reaction efficiency: reducing costs while also improving reaction efficiency, and can react completely in a C9 raw material in which methyl styrene, dicyclopentadiene and indene are mixed in a mass ratio. DETAILED DESCRIPTION

[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0039] Step 2: Add 1000g of the pretreated C9 fraction into the reactor and add 9g of BF 3 The catalyst and 1 g of the co-catalyst triisobutylaluminum were added dropwise in a metered manner, and after the addition was completed, stirring was continued to perform a preliminary reaction for 0.5 hours.

[0040] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0041] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0042] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0043] Example 2

[0044] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0045] Step 2: Add 1000g of the pretreated C9 fraction into the reactor and add 9g of BF 3 Catalyst, 1gAlCl 3 The catalyst was compounded and added dropwise in a measured manner. After the addition was completed, stirring was continued to perform a preliminary reaction for 0.5 hours.

[0046] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0047] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0048] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0049] Example 3

[0050] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0051] Step 2: Add 1000 g of the pretreated C9 fraction into the reactor and add 5 g of BF 3 Catalyst and 5gAlCl 3 The catalyst was compounded, and 1 g of the co-catalyst triisobutylaluminum was added dropwise in a metered manner. After the addition was completed, stirring was continued to perform a preliminary reaction for 0.5 hours.

[0052] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0053] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0054] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0055] Example 4

[0056] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0057] Step 2: Add 1000 g of the pretreated C9 fraction into the reactor and add 9 g of AlCl 3 The catalyst was compounded with 1 g of triisobutylaluminum catalyst and added dropwise in a metered manner. After the addition was completed, stirring was continued to perform a preliminary reaction for 0.5 hours.

[0058] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0059] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0060] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0061] Comparative Example 1

[0062] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0063] Step 2: Add 1000 g of the pretreated C9 fraction into the reactor, and continue stirring at 15° C. without adding any catalyst to conduct a pre-reaction for 0.5 h.

[0064] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0065] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0066] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0067] Comparative Example 2

[0068] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0069] Step 2: Add 1000g of the pretreated C9 fraction into the reactor and add 10g of BF 3 The catalyst was added dropwise in a metered manner, and after the addition was completed, stirring was continued to perform a preliminary reaction for 0.5 hours.

[0070] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0071] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0072] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0073] Comparative Example 3

[0074] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0075] Step 2: Add 1000 g of the pretreated C9 fraction into the reactor and add 10 g of AlCl 3 The catalyst was added dropwise in a metered manner, and after the addition was completed, stirring was continued to perform a preliminary reaction for 0.5 hours.

[0076] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0077] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0078] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0079] Comparative Example 4

[0080] Step 1: distill the raw materials to cut the light components and heavy components in the C9 fraction.

[0081] Step 2: Add 1000 g of the pretreated C9 fraction into the reactor, and add 10 g of the co-catalyst triisobutylaluminum dropwise in a metered manner at a temperature of 15° C. After the addition is completed, continue stirring to perform a pre-reaction for 0.5 hours.

[0082] Step 3: introduce nitrogen at a pressure of 0.5 MPa, raise the temperature to 40° C. and carry out polymerization reaction for 4 hours.

[0083] Step 4: After the reaction is completed, the temperature is lowered to room temperature, the polymer solution after the reaction is transferred to a neutralization kettle, and the pre-prepared liquid alkali is added to terminate the polymerization reaction. The polymerization solution is then washed with water until it is neutral to obtain a polymerization reaction solution.

[0084] Step 5: subjecting the polymerization reaction liquid to vacuum distillation to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance.

[0085] The preparation method of the C9 fraction pretreatment in Example 1-4 and Comparative Example 1-4 is as follows: the purchased ethylene cracking C9 raw material is put into a distillation kettle, the low temperature is controlled to be 90-100°C, the vacuum degree is 0.9-0.99Mpa, the reflux ratio is 1:20, the light components and heavy components in the ethylene cracking C9 are separated, and the main fraction at 120°C-200°C is collected. The main components are a mixed liquid of methyl styrene, dicyclopentadiene and indene.

[0086] The catalysts used in Examples 1-4 and Comparative Examples 1-4 and the experimental results are shown in Table 1:

[0087] Table 1: Resin test data results of the catalyst used in the experiment

[0088]

[0089] It can be seen from the above table that the molecular weight of the cold-polymerized resin provided in the embodiment of the present application is significantly narrower than that of the comparative example, and its toughness and heat resistance are higher than those of the comparative example, and it can maintain good performance under various environmental conditions; and its softening point is lower than that of the comparative example.

[0090] Although the present invention has been described in detail and some specific embodiments have been cited, it is obvious to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.

Claims

1. A method for preparing a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance, characterized in that: The steps are as follows: Step 1, distilling the C9 fraction to cut the light components and heavy components in the C9 fraction; Step 2: Add the pretreated C9 light component into the reactor, and add the compounded catalyst and co-catalyst dropwise in a metered manner at a temperature of 5-15°C, and continue stirring to perform a pre-reaction after the addition is completed; Step 3: introduce 0.1Mpa-0.5Mpa inert gas, raise the temperature to 30°C-40°C and carry out polymerization reaction for 3h-4h; Step 4: After the reaction is completed, the temperature is lowered to room temperature, and the polymer solution after the reaction is transferred to a neutralization kettle, and a pre-prepared liquid alkali is added to terminate the polymerization reaction; and then the polymer solution is washed with water until it is neutral to obtain a polymerization reaction solution; Step 5, distilling the polymerization reaction liquid under reduced pressure to remove oligomers, thereby obtaining a C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance; The total amount of the catalyst and the co-catalyst added is 0.5-1.5% of the mass of the reaction material; The percentage of the promoter in the reaction material is 0.05-0.2%.

2. The method for preparing a C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: The dropping time in step 2 is 0.1h-1h.

3. The method for preparing a C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: The liquid alkali in step 4 is one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution, and ammonia solution, and the concentration of the liquid alkali is 30wt%.

4. The method for preparing a C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: The temperature for removing oligomers by vacuum distillation in step 5 is 100°C-150°C, and the negative pressure condition is 700-1000 Pa.

5. A C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: The C9 raw material contains methyl styrene, dicyclopentadiene and indene components.

6. A C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: The catalyst is at least one of a BF3 complex catalyst, an AlCl3 catalyst, a boron trifluoride ether solution, and boron trifluoride.

7. A C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: The co-catalyst is at least one of triisobutylaluminum, molybdenum pentachloride and ethylaluminum dichloride.

8. A C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: The inert gas is nitrogen.

9. A C9 cold polymerization resin with narrow molecular weight, high toughness and good processing performance according to claim 1, characterized in that: In step 1, the C9 fraction is distilled to collect light components with a distillation range of 120-200°C.

10. A C9 cold-polymerized resin with narrow molecular weight, high toughness and good processing performance, characterized in that: Prepared by the method described in any one of claims 1 to 12.