High-strength PP film, preparation method thereof and composite current collector

High-strength PP films were prepared by blending and grafting PP with CBC, which solved the problem of insufficient tensile strength of PP films, achieved high-yield production of composite current collectors, and reduced production costs.

CN118909195APending Publication Date: 2024-11-08JIANGSU THREE LAYERS TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410984959.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing PP film has insufficient tensile strength at a thickness of 10μm in composite current collectors, resulting in low yield and high production cost during copper plating, which hinders the promotion and application of composite current collectors.

Method used

High-strength PP films were prepared by blending PP particles with CBC cyclic block copolymers and adding multifunctional and monofunctional vinyl monomers through grafting modification technology, thereby improving their tensile strength and reducing their elongation ratio.

Benefits of technology

High-strength PP film was successfully prepared with a tensile strength of over 380 MPa and a yield of 99.3%. It is suitable for composite current collector base film, reducing production costs and improving production yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004957122720000051
    Figure BDA0004957122720000051
  • Figure BDA0004957122720000052
    Figure BDA0004957122720000052
  • Figure BDA0004957122720000061
    Figure BDA0004957122720000061
Patent Text Reader

Abstract

The invention relates to the technical field of PP films, in particular to a high-strength PP film, a preparation method thereof and a composite current collector, and the high-strength PP film comprises the following components in parts by mass: 100 parts of PP, 5-15 parts of CBC, 0.3-3 parts of a multifunctional vinyl monomer, 0.5-6 parts of a monofunctional vinyl monomer and 0.1-1 part of a peroxide initiator. According to the high-strength PP film and the preparation method thereof disclosed by the invention, the composite current collector adopts a method of blending PP particles and CBC particles, the tensile strength of the PP film is improved by utilizing the CBC annular block copolymer, and meanwhile, the tensile strength of the PP film can be further improved and the reduction of the tensile ratio can be reduced by common grafting of two vinyl monomers; in addition, by adding the monofunctional vinyl monomer, the stretching rate can be further improved, so that a current collector base film which is stretched to the thickness of less than 10 microns is obtained, and the application of the composite current collector in a heat-resistant environment is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PP films, and in particular to a high-strength PP film and a preparation method thereof, and a composite current collector. Background Art

[0002] The composite current collector is a composite material that uses PET / PP and other raw material films as base films and deposits copper / aluminum molecules on both sides through processes such as vacuum coating. It adopts a three-layer composite structure of "metal-polymer material-metal", forms nano-scale metal on the surface of the polymer PET / PP film through vacuum evaporation, magnetron sputtering, etc., and then deposits the metal layer to thicken to more than 1μm through water electroplating.

[0003] Common types of plastic films include PET, PE, PVC, PP, PS, PC, PI, etc. Among them, PVC, PS, and PC are toxic and difficult to recycle, and are not suitable for use as substrates. Among the remaining plastics, polyethylene has a low tensile strength and may break when curled, so it is also not suitable for use as a substrate. PET has excellent electrical insulation, creep resistance, and fatigue resistance; PI has good heat resistance, resistance to extremely low temperatures, and excellent mechanical properties. PP has good heat resistance and electrical insulation, as well as a certain tensile strength, and is considered to be the most promising base film for composite current collectors.

[0004] However, the tensile strength of PP is lower than that of PET. The thickness of the base film suitable for the current collector is generally in the range of 4.5±1μm. Under this thickness condition, the PP base film is easily broken, resulting in serious impact on the yield during the copper plating process. The current production yield is about 20-40%, which greatly increases the production cost and hinders the promotion and application of composite current collectors.

[0005] Therefore, how to solve the problem of insufficient tensile strength of PP film in a composite current collector with a thickness of 10 μm is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0006] The present invention provides a high-strength PP film and a preparation method thereof, and a composite current collector, so as to solve the problem that the tensile strength of the existing PP film in a 10 μm thickness environment is not suitable for a base film in a composite current collector.

[0007] In order to solve the above technical problems, the present invention provides a high-strength PP film, comprising the following components in parts by weight: 100 parts of PP, 5-15 parts of CBC, 0.3-3 parts of multifunctional vinyl monomers, 0.5-6 parts of monofunctional vinyl monomers, and 0.1-1 parts of peroxide initiators.

[0008] Furthermore, the multifunctional vinyl monomer includes any one or more combinations of TAIC, TMPTA, ethoxylated TMPTA, propoxylated TMPTA, vinyl cyclotetrasiloxane, bisvinyl-terminated dimethylsilane, hexanediol di(meth)acrylate, butanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate.

[0009] Furthermore, the multifunctional vinyl monomer is preferably a combination of bisvinyl-terminated dimethylsiloxane and vinylcyclotetrasiloxane.

[0010] Furthermore, the monofunctional vinyl monomer includes any one or more combinations of KH570, 171 silane coupling agent, 151 silane coupling agent, butyl (meth)acrylate, isooctyl (meth)acrylate, and vinyl acetate.

[0011] Furthermore, the longitudinal tensile strength of the high-strength PP film is not less than 380 MPa, and the transverse tensile strength is not less than 280 MPa.

[0012] Furthermore, the yield rate of the high-strength PP film after stretching is not less than 99.3%.

[0013] On the other hand, the present invention also provides a method for preparing the high-strength PP film as described above, comprising the following steps: step S1, grafting and modifying PP, CBC, a multifunctional vinyl monomer, a monofunctional vinyl monomer and a peroxide initiator and granulating them to obtain grafted particles; step S2, casting and extruding the grafted particles into a film to obtain a high-strength PP film.

[0014] Furthermore, the grafting temperature in step S1 is not higher than 200°C.

[0015] In a third aspect, the present invention further provides a composite current collector, comprising: a base film and a metal layer deposited on both sides of the base film; wherein the base film is the high-strength PP film as described above.

[0016] Furthermore, the thickness of the base film is 4.5±1 μm.

[0017] The beneficial effects of the present invention are that the high-strength PP film and its preparation method, and the composite current collector of the present invention adopt a method of blending PP particles and CBC particles, and use CBC cyclic block copolymers to improve the tensile strength of the PP film. At the same time, the co-grafting of two vinyl monomers can further improve the tensile strength of the PP film while reducing the reduction in the stretching ratio. In addition, the addition of monofunctional vinyl monomers can further increase the stretching ratio, thereby obtaining a current collector base film that is stretched to a thickness of less than 10 μm, thereby realizing the application of the composite current collector in a heat-resistant environment.

[0018] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description.

[0019] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below for detailed description as follows. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] At least one embodiment provides a high-strength PP film, comprising the following components in parts by weight: 100 parts of PP, 5-15 parts of CBC, 0.3-3 parts of multifunctional vinyl monomer, 0.5-6 parts of monofunctional vinyl monomer, and 0.1-1 parts of peroxide initiator.

[0022] In some embodiments, the PP is polypropylene.

[0023] In some embodiments, the CBC is fully hydrogenated SBS, which is a cyclic block copolymer, preferably Taiwan Taiju CBC resin produced by Taiju Corporation.

[0024] In some embodiments, the multifunctional vinyl monomer includes any one or more combinations of TAIC, TMPTA, ethoxylated TMPTA, propoxylated TMPTA, vinyl cyclotetrasiloxane, bisvinyl-terminated dimethylsilane, hexanediol di(meth)acrylate, butanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate.

[0025] In some embodiments, the multifunctional vinyl monomer is preferably a combination of bis-vinyl-terminated dimethylsiloxane and vinyl cyclotetrasiloxane, because both ends of the siloxane are soft, which can reduce the degree of rate reduction.

[0026] In some embodiments, the monofunctional vinyl monomer includes any one or more combinations of KH570, 171 silane coupling agent, 151 silane coupling agent, butyl (meth)acrylate, isooctyl (meth)acrylate, and vinyl acetate.

[0027] In some embodiments, the peroxide initiator is preferably bis-25, ie, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

[0028] At least one embodiment provides a method for preparing a high-strength PP film as described above, comprising the following steps: step S1, grafting and modifying PP, CBC, a multifunctional vinyl monomer, a monofunctional vinyl monomer and a peroxide initiator and granulating them to obtain grafted particles; step S2, casting and extruding the grafted particles into a film to obtain a high-strength PP film.

[0029] In some embodiments, the grafting temperature in step S1 is not higher than 200°C.

[0030] At least one embodiment provides a composite current collector, comprising: a base film and a metal layer deposited on both sides of the base film; wherein the base film is the high-strength PP film as described above.

[0031] In some embodiments, the base film has a thickness of 4.5±1 μm.

[0032] In some embodiments, PP films were prepared by mixing 100 parts of PP with several parts of blended particles to obtain the composition and performance data of each embodiment 1-7 as shown in Table 1 below, wherein the blended particles are CBC and other comparative particles with similar performance to CBC.

[0033] Table 1

[0034]

[0035] In this embodiment, specifically, as can be seen from Table 1 above, the CBC cyclic block copolymer can improve the tensile strength of the PP film. Since the stretching ratio is limited, the addition amount is preferably 5-15 parts.

[0036] In this embodiment, specifically, a peroxide initiator and a grafting monomer are added according to PP:CBC=100 parts:10 parts, wherein the initiator is 0.5 parts of bis-25, and the grafting monomer is a multifunctional vinyl monomer, such as TAIC, TMPTA, ethoxylated TMPTA, propoxylated TMPTA, hexanediol diacrylate, etc., and grafting modification is carried out at 200°C to obtain the components and performance data of each embodiment in Examples 8-24 shown in Table 2 below.

[0037] Table 2

[0038]

[0039]

[0040] As shown in Table 2 above, grafting multifunctional vinyl monomers can improve the tensile strength of PP film, but it will also reduce the stretch ratio, so the addition amount is preferably 0.3-3 parts. Among them, divinyl-terminated dimethylsiloxane has the best comprehensive effect, followed by vinyl cyclotetrasiloxane, mainly because the two ends of siloxane are soft, which reduces the degree of reduction in ratio.

[0041] In some embodiments, a peroxide initiator and a grafting monomer are added according to PP:CBC=100 parts:10 parts, wherein the initiator is 0.5 parts of Bis-25, and grafting modification is carried out at 200°C to obtain the components and performance data of each embodiment of Examples 25-30 shown in Table 3 below.

[0042] Table 3

[0043]

[0044] It can be seen from Table 3 above that the two vinyl silanes assist each other and can further improve the tensile strength of the PP film while reducing the reduction in the stretch ratio.

[0045] In some embodiments, a peroxide initiator and a grafting monomer are added according to the ratio of PP:CBC:vinyl cyclotetrasiloxane:bisvinyl-terminated dimethylsiloxane = 100 parts: 10 parts: 1 part: 1 part, wherein the initiator is 0.5 parts of bis-25, and grafting modification is carried out at 200° C. to obtain the components and performance data of each embodiment of Examples 31-39 shown in Table 4 below.

[0046] Table 4

[0047]

[0048] It can be seen from Table 4 above that the addition of monofunctional vinyl monomers can increase the stretching ratio of PP film, but it will also reduce the longitudinal and transverse tensile strength. Therefore, the combination of monofunctional vinyl monomers and multifunctional vinyl monomers within an appropriate range can increase the stretching ratio and thus the tensile strength.

[0049] In some embodiments, the high-strength PP film has a longitudinal tensile strength of not less than 380 MPa, and a transverse tensile strength of not less than 280 MPa.

[0050] In some embodiments, the yield rate of the high-strength PP film after stretching is not less than 99.3%.

[0051] The post-processing yields in Tables 1 to 4 above refer to the processing yields after stretching.

[0052] In summary, the high-strength PP film and its preparation method, and the composite current collector adopt a method of blending PP particles and CBC particles, and use CBC cyclic block copolymers to improve the tensile strength of the PP film. At the same time, the co-grafting of two vinyl monomers can further improve the tensile strength of the PP film while reducing the reduction in the stretching ratio. In addition, the addition of monofunctional vinyl monomers can further increase the stretching ratio, thereby obtaining a current collector base film that is stretched to a thickness of less than 10μm, thereby realizing the application of the composite current collector in a heat-resistant environment.

[0053] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A high-strength PP film, characterized in that: The invention comprises the following components in parts by weight: 100 parts of PP, 5-15 parts of CBC, 0.3-3 parts of multifunctional vinyl monomer, 0.5-6 parts of monofunctional vinyl monomer and 0.1-1 parts of peroxide initiator.

2. The high-strength PP film according to claim 1, characterized in that: The multifunctional vinyl monomer includes any one or more combinations of TAIC, TMPTA, ethoxylated TMPTA, propoxylated TMPTA, vinyl cyclotetrasiloxane, bisvinyl-terminated dimethylsilane, hexanediol di(meth)acrylate, butanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate.

3. The high-strength PP film according to claim 1, characterized in that: The multifunctional vinyl monomer is preferably a combination of bisvinyl-terminated dimethylsiloxane and vinylcyclotetrasiloxane.

4. The high-strength PP film according to claim 1, characterized in that: The monofunctional vinyl monomer includes any one or more combinations of KH570, 171 silane coupling agent, 151 silane coupling agent, butyl (meth)acrylate, isooctyl (meth)acrylate, and vinyl acetate.

5. The high-strength PP film according to claim 1, characterized in that: The longitudinal tensile strength of the high-strength PP film is not less than 380 MPa, and the transverse tensile strength is not less than 280 MPa.

6. The high-strength PP film according to claim 1, characterized in that: The yield rate of the high-strength PP film after stretching is not less than 99.3%.

7. A method for preparing a high-strength PP film according to any one of claims 1 to 6, characterized in that: The steps include: Step S1, grafting and modifying PP, CBC, multifunctional vinyl monomer, monofunctional vinyl monomer and peroxide initiator and granulating to obtain grafted particles; Step S2, casting and extruding the grafted particles into a film to obtain a high-strength PP film.

8. The method for preparing a high-strength PP film according to claim 7, characterized in that: The grafting temperature in step S1 is not higher than 200°C.

9. A composite current collector, characterized in that: include: A base film and a metal layer deposited on both sides of the base film; in The base film is a high-strength PP film as described in any one of claims 1-6.

10. The composite current collector according to claim 9, characterized in that: The thickness of the base film is 4.5±1 μm.

Citation Information

Cited By

  • High-strength low-elongation bipolar current collector and preparation method thereof

    CN119725547A