Oil well cement paste retarder as well as preparation method and application thereof
By preparing an oil well cement slurry retarder composed of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methylallyl polyoxyethylene ether, the existing technology is solved under high temperature and high pressure conditions. The problem of poor performance has achieved efficient cementing in deep and ultra-deep wells, with good temperature adaptability and compressive strength.
Patent Information
- Application Number
- CN202411417144.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The cement retarder of existing oil wells has poor performance under high temperature and high pressure conditions, resulting in the construction quality of deep wells and ultra-deep wells not meeting the standards and the cost is high.
The reaction was carried out by mixing 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methylallyl polyoxyethylene ether in deionized water, adding a pH adjuster and an initiator, and the reaction was washed and dried , grinding, and preparing a high temperature-resistant oil well cement slurry retarder.
This retarder can delay cement hydration reaction, extend the settling time, and decomposition temperature up to 365℃, maintain compressive strength at low temperatures, have good temperature adaptability and compatibility, and meet the cementing needs under high temperature and high pressure conditions.
Smart Images

Figure CN118909205A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil well cement admixtures, in particular to an oil well cement slurry retarder and a preparation method and application thereof. Background Art
[0002] Oil is a vital component of the energy industry. In recent years, with increasing oil consumption, oil extraction efforts have intensified. Shallow reserves cannot meet the demand for oil and natural gas; however, to achieve this goal, new oil and gas resources can be developed at greater depths. Therefore, more advanced extraction technologies are needed to access deep oil and gas and improve extraction efficiency. Currently, cementing both domestically and internationally faces challenges such as safe pumping under high temperature and pressure, slow cement top growth, poor compatibility, and abnormal thickening curves, resulting in substandard cementing quality.
[0003] Currently, lignin sulfonates, hydroxyethyl cellulose, hydroxycarboxylic acids (tartaric acid, citric acid, and sodium gluconate), and polymer retarders are the main types of retarders used in the cementing industry. Lignosulfonates are a widely used type due to their diverse raw material sources. However, their retarding effect is not ideal when used at temperatures above 100°C. The thickening effect of hydroxyethyl cellulose retarders often affects the rheological properties of cement slurries. Hydroxycarboxylic acid retarders, such as sodium gluconate and tartaric acid, are frequently used in deep wells due to their low cost. However, hydroxycarboxylic acid retarders have the disadvantage of being dosage-sensitive and often leading to abnormal setting problems. For example, the most widely studied and applied retarder for cement slurry expansion is polymer retarders. Unlike other types of retarders, polymer retarders can be synthesized and designed at the molecular level, and functional groups with superior performance can be introduced under desired formation conditions to enhance the polymer's retarding ability. Due to their tunable properties, polymer admixtures have become increasingly popular in cementing projects in recent years.
[0004] While oilfield admixtures are widely used in oilfield development, both domestically and internationally, they still suffer from drawbacks such as poor performance and high costs. Compared to foreign products, most domestic products can meet certain cementing requirements at medium to high temperatures (90°C to 120°C), but few retarders are suitable for use in high-temperature, high-pressure oil and gas wells found in deep and ultra-deep wells. Therefore, developing a retarder that is resistant to high temperatures and has a wide range of applications is key to improving cementing quality in deep and ultra-deep wells and holds significant potential for future application. Summary of the Invention
[0005] The present invention provides an oil well cement slurry retarder and a preparation method and application thereof, which overcome the deficiencies of the above-mentioned prior art and can effectively solve the problem of poor high temperature resistance of the existing retarders.
[0006] One of the technical solutions of the present invention is achieved by the following measures: an oil well cement slurry retarder is prepared according to the following steps: In the first step, required amounts of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid, and methyl allyl polyoxyethylene ether are mixed and dissolved in deionized water, and a pH regulator is added to obtain a mixed solution; In the second step, the mixture is stirred and nitrogen is introduced, and then a required amount of initiator is added. After heating for reaction, stirring and heating are stopped, and the mixture is cooled to room temperature to obtain a reaction product. The third step is to wash, filter, dry and grind the reaction product to obtain an oil well cement slurry retarder.
[0007] The following is a further optimization and / or improvement of one of the above-mentioned technical solutions: In the first step, the mass ratio of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methallyl polyoxyethylene ether added is 5 to 6:2 to 3:1 to 2.
[0008] In the first step, the pH adjuster is a sodium hydroxide solution with a mass concentration of 30%, and the pH value of the mixed solution is 5 to 7.
[0009] In the second step, the stirring speed is 200 r / min to 400 r / min, and the nitrogen introduction time is 15 min to 30 min.
[0010] In the second step, the amount of the initiator added is 0.2% to 0.4% of the total mass of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methyl allyl polyoxyethylene ether.
[0011] The initiator is a mixture of potassium persulfate and sodium bisulfite in a mass ratio of 1:1.
[0012] In the above second step, the heating temperature is 60° C. to 80° C., and the reaction time is 5 h to 6 h.
[0013] In the third step, the washing liquid for washing the reaction product is ethanol with a volume 3 to 5 times that of the reaction product, and the drying condition is vacuum drying at 50° C. to 80° C.
[0014] The second technical solution of the present invention is achieved by the following measures: A method for preparing an oil well cement slurry retarder is carried out according to the following steps: In the first step, required amounts of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid, and methyl allyl polyoxyethylene ether are mixed and dissolved in deionized water, and a pH regulator is added to obtain a mixed solution; In the second step, the mixture is stirred and nitrogen is introduced, and then a required amount of initiator is added. After heating for reaction, stirring and heating are stopped, and the mixture is cooled to room temperature to obtain a reaction product. The third step is to wash, filter, dry and grind the reaction product to obtain an oil well cement slurry retarder.
[0015] The third technical solution of the present invention is achieved through the following measures: an oil well cement slurry retarder is used in high-temperature cementing.
[0016] The oil well cement slurry retarder of the present invention can delay the cement hydration reaction, thereby extending the cement setting time and providing protection for cementing safety. Not only does it have a decomposition temperature as high as 365°C in a thermal gravimetric test, it can also ensure the development of the compressive strength of the cement slurry at low temperatures and has good temperature adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Attachment Figure 1 This is the thermogravimetric diagram of the oil well cement slurry retarder of the present invention.
[0018] Attachment Figure 2 This is a thickening curve of the oil well cement slurry retarder of the present invention at 120°C and 60 MPa.
[0019] Attachment Figure 3 This is a thickening curve of the oil well cement slurry retarder of the present invention at 150°C and 90 MPa. DETAILED DESCRIPTION
[0020] The present invention is not limited to the following embodiments, and specific implementation methods can be determined based on the technical solutions of the present invention and actual conditions. Unless otherwise specified, the various chemical reagents and chemicals mentioned in the present invention are all chemical reagents and chemicals commonly known in the prior art; unless otherwise specified, the percentages in the present invention are all percentages by mass; unless otherwise specified, the solutions in the present invention are all aqueous solutions with water as the solvent, for example, hydrochloric acid solution is an aqueous hydrochloric acid solution; normal temperature and room temperature in the present invention generally refer to temperatures between 15°C and 25°C, and are generally defined as 25°C.
[0021] The present invention will be further described below in conjunction with the embodiments: Example 1: The oil well cement slurry retarder is prepared according to the following steps: In the first step, the required amount of 2-acrylamide-2-methylpropanesulfonic acid (AMPS), maleic acid (MA) and methyl allyl polyoxyethylene ether (TPEG-2400) were mixed and dissolved in deionized water, and a pH regulator was added to obtain a mixed solution. The mixed solution was 100 mL. In the second step, the mixed solution is poured into a reactor, stirred and introduced with nitrogen, and then a required amount of initiator is added. After heating for reaction, stirring and heating are stopped, and the mixture is cooled to room temperature to obtain a reaction product. In the third step, the reaction product is washed and filtered, cut into small pieces with scissors, dried and ground to obtain white microsphere powder (i.e., oil well cement slurry retarder).
[0022] The oil well cement slurry retarder of the present invention is obtained by copolymerizing 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methyl allyl polyoxyethylene ether. The thermogravimetric test shows that the retarder has a decomposition temperature of up to 365°C. In addition, the retarder can ensure the development of the compressive strength of the cement slurry at low temperatures, has good temperature adaptability, and has good compatibility and dispersibility with the G33S water reducer.
[0023] Methyl allyl polyoxyethylene ether (TPEG-2400) is beneficial to the strength development of cement paste at lower temperatures because it has a large number of side groups that can wrap around and encapsulate cement particles, and then wrap and stretch them according to temperature changes. In addition, maleic acid MA monomer can react with Ca 2+ The combination creates a chelate, which can help the cement hydrate more slowly. The sulfonic acid groups of the AMPS monomers have high thermal stability.
[0024] The retarder of this invention uses methyl allyl polyoxyethylene ether (TPEG-2400) as a polymerizable monomer, which facilitates the development of cement slurry strength at lower temperatures. TPEG has numerous pendant groups that can wrap around and encapsulate cement particles, subsequently encapsulating and stretching them in response to temperature fluctuations. Furthermore, the MA monomer can combine with Ca2+ to form a chelate, which helps the cement hydrate more slowly. The sulfonic acid group of the AMPS monomer has high thermal stability. The addition of MA and AMPS introduces carboxyl and sulfonic acid groups, enhancing the retarder's adsorption capacity under high-temperature conditions.
[0025] The ternary polymer formed by copolymerizing 2-acrylamide-2-methylpropanesulfonic acid (AMPS), maleic acid (MA) and methyl allyl polyoxyethylene ether (TPEG-2400) has good temperature resistance and good retarding performance at 150°C. At the same time, the cement slurry has good rheological properties and does not affect the compressive strength of the cement paste.
[0026] Example 2: As an optimization of the above example, in the first step, the mass ratio of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methallyl polyoxyethylene ether added is 5 to 6:2 to 3:1 to 2.
[0027] Example 3: As an optimization of the above example, in the first step, the pH regulator is a sodium hydroxide solution with a mass concentration of 30%, and the pH value of the mixed solution is 5 to 7.
[0028] Example 4: As an optimization of the above example, in the second step, the stirring speed is 200 r / min to 400 r / min, and the nitrogen introduction time is 15 min to 30 min.
[0029] Example 5: As an optimization of the above example, in the second step, the amount of initiator added is 0.2% to 0.4% of the total mass of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methallyl polyoxyethylene ether.
[0030] Example 6: As an optimization of the above example, the initiator is a mixture of potassium persulfate and sodium bisulfite in a mass ratio of 1:1.
[0031] Example 7: As an optimization of the above example, in the second step, the heating temperature is 60°C to 80°C, and the reaction time is 5h to 6h.
[0032] Example 8: As an optimization of the above example, in the third step, the washing liquid for washing the reaction product is ethanol with a volume 3 to 5 times that of the reaction product, and the drying condition is vacuum drying at 50°C to 80°C.
[0033] Example 9: The preparation method of the oil well cement slurry retarder is carried out according to the following steps: In the first step, required amounts of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid, and methyl allyl polyoxyethylene ether are mixed and dissolved in deionized water, and a pH regulator is added to obtain a mixed solution; In the second step, the mixture is stirred and nitrogen is introduced, and then a required amount of initiator is added. After heating for reaction, stirring and heating are stopped, and the mixture is cooled to room temperature to obtain a reaction product. The third step is to wash, filter, dry and grind the reaction product to obtain an oil well cement slurry retarder.
[0034] Example 10: Application of the oil well cement slurry retarder in high-temperature well cementing.
[0035] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The oil well cement slurry retarder of the present invention has a wide range of applications. It is not only superior to traditional AMPS retarders in terms of temperature resistance, but also has good temperature adaptability.
[0036] (2) The oil well cement slurry retarder of the present invention has significant retarding performance at 150°C and a smooth thickening curve. It can ensure the development of the compressive strength of the cement slurry at low temperatures, has good temperature adaptability, and has good compatibility and dispersibility with the G33S water reducer.
[0037] Example 11: The oil well cement slurry retarder is prepared according to the following steps: In the first step, in a 250-ml four-necked flask equipped with a stirrer, a condenser, a thermometer, and 100 ml of deionized water, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), maleic acid (MA), and methyl allyl polyoxyethylene ether (TPEG-2400) were mixed and dissolved in a mass ratio of 6:2.5:1.5. A pH adjuster (30% sodium hydroxide solution) was then added to obtain a mixed solution, and the pH of the mixed solution was adjusted to 6. In the second step, the mixed solution was poured into a reactor, stirred at a speed of 300 r / min and nitrogen was introduced for 30 minutes, and then an initiator (a mixture of ammonium persulfate and sodium bisulfite with a mass ratio of 1:1) with a total weight of 0.2% of 2-acrylamide-2-methylpropanesulfonic acid (AMPS), maleic acid (MA) and methyl allyl polyoxyethylene ether (TPEG-2400) was added. The mixture was heated to 60°C for 6 hours (maintaining constant temperature), and then stirring and heating were stopped, and the mixture was cooled to room temperature to obtain a reaction product. In the third step, the reaction product was washed with 3 times the volume of ethanol, filtered, cut into small pieces with scissors, placed in a vacuum drying oven at 50°C and dried to constant weight, and ground to obtain white microsphere powder (i.e., oil well cement slurry retarder).
[0038] Example 12: The oil well cement slurry retarder is prepared according to the preparation method described in Example 11: In the first step, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), maleic acid (MA), and methyl allyl polyoxyethylene ether (TPEG-2400) were mixed and dissolved in a mass ratio of 5.5:2.5:2 in a 250-ml four-necked flask equipped with a stirrer, a condenser, a thermometer, and 100 ml of deionized water. A pH adjuster (30% sodium hydroxide solution) was then added to obtain a mixed solution, and the pH of the mixed solution was adjusted to 7. In the second step, the mixed solution was poured into a reactor, stirred at a speed of 300 r / min and nitrogen was introduced for 30 minutes, and then an initiator (a mixture of ammonium persulfate and sodium bisulfite with a mass ratio of 1:1) with a total weight of 0.4% of 2-acrylamide-2-methylpropanesulfonic acid (AMPS), maleic acid (MA) and methyl allyl polyoxyethylene ether (TPEG-2400) was added. The mixture was heated to 60°C for 6 hours (maintaining constant temperature), and then stirring and heating were stopped, and the mixture was cooled to room temperature to obtain a reaction product. In the third step, the reaction product was washed with 4 times the volume of ethanol, filtered, cut into small pieces with scissors, placed in a vacuum drying oven at 50°C and dried to constant weight, and ground to obtain white microsphere powder (i.e., oil well cement slurry retarder).
[0039] Experimental Example 1: Compatibility test of the oil well cement slurry retarder obtained in Example 11 with other additives: The formula of the cement slurry system in the compatibility experiment is: 600g of G-grade high-resistance cement + 2% fluid loss reducer G33S + 4% retarder + 35% quartz sand + 0.5% dispersant SXY-2 + 0.44% tap water.
[0040] In this experimental example, the fluid loss additive G33 and the dispersant SXY are commercially available products, and the retarder is the oil well cement slurry retarder prepared in Example 11.
[0041] The thermogravimetric graph of the oil well cement slurry retarder prepared in Example 11 of the present invention is as follows: Figure 1 As shown. Figure 1 It can be seen that the decomposition temperature of the oil well cement slurry retarder of the present invention is as high as 365°C.
[0042] Experimental Example 2: Compatibility test of the oil well cement slurry retarder obtained in Example 12 with other additives: The formula of the cement slurry system in the cement slurry rheology test is: 600g of G-grade high-resistance cement + 3% retarder + 35% quartz sand + 0.5% dispersant SXY-2 + 0.44% tap water.
[0043] In this experimental example, the dispersant SXY is a commercially available product, and the retarder is the oil well cement slurry retarder prepared in Example 12.
[0044] The performance of the above experimental examples 1 and 2 was verified: (1) Compatibility test of the oil well cement slurry retarder obtained in Example 11 of the present invention with other additives A high-temperature and high-pressure thickener was used to measure the cement slurry at 120°C and 60MPa (using the formulation of the cement slurry system described in Experimental Example 1) as a benchmark, and the experimental conditions for the water loss experiment were 120°C and 60MPa. The amount of the obtained oil well cement slurry retarder was adjusted to study the compatibility with other additives at different amounts of oil well cement slurry retarder. The amounts of oil well cement slurry retarder in the experiment were set to 0%, 0.5%, 1%, 1.5%, 2%, and 2.5%, respectively. The results are shown in Table 1. It can be seen from Table 1 that with the increase in the amount of oil well cement slurry retarder, there is a good linear relationship between the thickening time and water loss of the cement slurry and the amount of oil well cement slurry retarder. It has good compatibility with G33S and SXY, and meets the needs of cementing operations under different environments. Among them, the thickening curve at 2% oil well cement slurry retarder is as follows Figure 2 As shown ( Figure 2 The three vertical axes in the chart represent temperature, pressure and consistency value from left to right). Figure 2 It can be seen that at 120°C, the cement slurry has significant retarding properties, a smooth thickening curve, and no abnormal phenomena such as "bulges" or "steps". The thickening time meets the safety standards of high-temperature pumps and meets the needs of cementing operations under high-temperature conditions.
[0045] (2) High temperature resistance and slow setting performance The dosage of the oil well cement slurry retarder obtained in Example 11 of the present invention was varied, and the thickening time of the cement slurry (using the cement slurry system formulation described in Experimental Example 1) at 150°C and 90 MPa was tested using a high-temperature and high-pressure thickener. The results are shown in Table 2. As can be seen from Table 2, at 150°C and 90 MPa, when the dosage of the oil well cement slurry retarder was 4%, the thickening time was 365 minutes. The thickening curve at the 4% dosage of the oil well cement slurry retarder is shown in Figure 2. Figure 3 As shown ( Figure 3 The three vertical axes in the chart represent temperature, pressure and consistency value from left to right). Figure 3 It can be seen that at 150°C, the cement slurry has significant retarding properties, a smooth thickening curve, and no abnormal phenomena such as "bulges" or "steps." The thickening time meets the safety standards for high-temperature pumps and meets the requirements of cementing operations under high-temperature conditions.
[0046] (3) Compressive strength of cement paste at different temperatures and dosages A cubic mold was filled with prefabricated cement slurry. The finished mold was placed in a curing chamber and allowed to rest for 24 hours. The compressive strength of the cement paste was tested using a universal testing machine. The compressive strength of the cement slurry (using the cement slurry system described in Experimental Example 2) at different curing temperatures is shown in Table 3.
[0047] As shown in Table 3, with the increase in the amount of the oil well cement slurry retarder obtained in Example 12 of the present invention, the compressive strength of the cement paste decreases. However, at 90°C and with a 3% amount of the oil well cement slurry retarder added, the compressive strength of the cement is still greater than 14 MPa, meeting the requirements of the cementing task.
[0048] In summary, the oil well cement slurry retarder of the present invention can delay the cement hydration reaction, thereby extending the cement setting time and providing protection for cementing safety. Not only does it have a decomposition temperature as high as 365°C in the thermal gravimetric test, it can also ensure the development of the compressive strength of the cement slurry at low temperatures and has good temperature adaptability.
[0049] The above technical features constitute the embodiments of the present invention, which have strong adaptability and implementation effect. Non-essential technical features can be added or removed according to actual needs to meet the requirements of different situations.
[0050] Table 1 .
[0051] Table 2 .
[0052] Table 3 .
Claims
1. An oil well cement slurry retarder, characterized in that Prepared according to the following steps: The first step is to mix and dissolve the required amount of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methyl allyl polyoxyethylene ether in deionized water, and then add a pH regulator to obtain a mixed solution; The second step is to stir the mixed solution and introduce nitrogen, then add the required amount of initiator, heat to react, stop stirring and heating, and cool to room temperature to obtain a reaction product; The third step is to wash, filter, dry and grind the reaction product to obtain an oil well cement slurry retarder.
2. The oil well cement slurry retarder according to claim 1, characterized in that In the first step, the mass ratio of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methyl allyl polyoxyethylene ether added is 5 to 6:2 to 3:1 to 2.
3. The oil well cement slurry retarder according to claim 1 or 2, characterized in that In the first step, the pH adjuster is a sodium hydroxide solution with a mass concentration of 30%, and the pH value of the mixed solution is 5 to 7.
4. The oil well cement slurry retarder according to claim 3, characterized in that In the second step, the stirring speed is 200 r / min to 400 r / min, and the nitrogen introduction time is 15 min to 30 min.
5. The oil well cement slurry retarder according to claim 1, 2 or 4, characterized in that In the second step, the amount of initiator added is 0.2% to 0.4% of the total mass of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methyl allyl polyoxyethylene ether.
6. The oil well cement slurry retarder according to claim 5, characterized in that The initiator is a mixture of potassium persulfate and sodium bisulfite in a mass ratio of 1:
1.
7. The oil well cement slurry retarder according to claim 6, characterized in that In the second step, the heating temperature is 60°C to 80°C, and the reaction time is 5h to 6h.
8. The oil well cement slurry retarder according to claim 1, 2, 4, 6 or 7, characterized in that In the third step, the washing liquid for washing the reaction product is ethanol in a volume 3 to 5 times that of the reaction product, and the drying condition is vacuum drying at 50° C. to 80° C.
9. A method for preparing an oil well cement slurry retarder according to any one of claims 2 to 8, characterized in that Follow the steps below: The first step is to mix and dissolve the required amount of 2-acrylamide-2-methylpropanesulfonic acid, maleic acid and methyl allyl polyoxyethylene ether in deionized water, and then add a pH regulator to obtain a mixed solution; The second step is to stir the mixed solution and introduce nitrogen, then add the required amount of initiator, heat to react, stop stirring and heating, and cool to room temperature to obtain a reaction product; The third step is to wash, filter, dry and grind the reaction product to obtain an oil well cement slurry retarder.
10. Use of the oil well cement slurry retarder according to any one of claims 1 to 8 in high temperature cementing.
Citation Information
Patent Citations
A polycarboxylate superplasticizer with high water reduction rate and high slump retention, its synthesis method and application method
CN102268121A
Preparation method of super-retarding type polycarboxylate superplasticizer
CN103848944A
High-temperature-resistant copolymer oil well cement retarder and preparation method thereof
CN104403056A
Preparation method of temperature-adaptive retarder
CN106699989A
Super-retarded concrete and preparation method thereof
CN109400050A