Thermoplastic resin, preparation method thereof and reinforced fiber composite material

By introducing specific molecular structures and catalysts into thermoplastic resins, the mechanical properties and environmental impact of thermosetting resins in reinforcing fiber composite materials are solved, and the preparation of high-performance thermoplastic resins and reinforcing fiber composite materials is realized, which improves the material Mechanical properties and environmental protection.

CN118909240APending Publication Date: 2024-11-08TEN TECH COMPOSITE TECH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410988624.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The application of existing thermosetting resins in reinforced fiber composite materials has problems such as insufficient mechanical strength, poor impact performance and unrecyclable, which affects the environment and processing efficiency.

Method used

A thermoplastic resin has been developed, which contains specific segments in its molecular structure, which promotes polymerization reaction generation through catalysts, has excellent mechanical properties and reinforced fiber surface adhesion effect, and is used to prepare high-performance reinforced fiber composite materials.

Benefits of technology

The mechanical properties and interface peel strength of thermoplastic resins are improved, the overall performance of reinforced fiber composites is enhanced, and the environmental impact of the production process is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909240A_ABST
    Figure CN118909240A_ABST
Patent Text Reader

Abstract

The invention provides a thermoplastic resin, the molecular structure of the thermoplastic resin comprises a chain segment shown in the following general formula I, the general formula I is # imgabs0 #, in the general formula I, Ar1 and Ar2 are independently selected from aromatic groups containing benzene rings, R is alkyl, and n is the degree of polymerization of the general formula I; the weight-average molecular weight of the thermoplastic resin is more than 40000, and the glass transition temperature of the thermoplastic resin is 85-130 DEG C. The thermoplastic resin provided by the invention has good bending strength, compression strength and impact property after being cured and molded, and also has good acid and alkali resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer materials, and in particular, relates to a thermoplastic resin and a preparation method thereof, and a reinforced fiber composite material. Background Art

[0002] Reinforced fiber composite materials composed of reinforcing fibers and resins are widely used in various industries such as automotive parts, sports equipment, aerospace, etc. due to their excellent mechanical properties. In order to further improve the mechanical properties of reinforced fiber composite materials, the most direct way is to increase the content of reinforcing fibers in the composite materials. However, as the content of reinforcing fibers increases, it is difficult for the reinforcing fibers to be evenly distributed in the resin, which leads to a decrease in the impact strength of the reinforced fiber composite materials. In view of this, it is necessary to seek other technical means to improve the mechanical properties of reinforced fiber composite materials, such as using resins with excellent mechanical properties to composite with reinforcing fibers. Based on the characteristics of thermosetting materials with low viscosity, high strength, good rigidity, excellent weather resistance and heat resistance, and good composite impregnation of thermosetting resins and reinforcing fibers, and convenient processing, the reinforced fiber composite materials on the market are mainly composed of thermosetting resins and reinforcing fibers. However, thermosetting resins cannot be recycled, need to be formed once, and have a long processing cycle, a post-ripening process, large pollution during operation, and a large impact on the environment. Thermoplastic resins are widely used in automobiles, home appliances, electronic appliances, machinery and other fields due to their excellent molding and processing performance, heat resistance, dimensional stability and other advantages. However, thermoplastic resins often have defects such as insufficient mechanical strength and poor impact resistance during use. The existence of these problems constitutes an obstacle to the application of thermoplastic resins in reinforced fiber composite materials. Summary of the invention

[0003] In order to improve the mechanical properties of a thermoplastic resin, the present invention provides a thermoplastic resin and a preparation method thereof.

[0004] According to a first aspect of the present invention, a thermoplastic resin is provided, wherein the molecular structure of the thermoplastic resin comprises a chain segment represented by the following general formula I: In general formula I, Ar1 and Ar2 are independently selected from aromatic groups containing benzene rings, R is a hydrocarbon group, and n is the degree of polymerization of general formula I; the weight average molecular weight of the thermoplastic resin is above 40,000, and the glass transition temperature of the thermoplastic resin is 85-130°C. The thermoplastic resin provided by the present invention has excellent mechanical properties after curing and molding. In addition, the above-mentioned thermoplastic resin has a good surface adhesion effect on the reinforcing fiber. Based on this, the raw materials for preparing the above-mentioned thermoplastic resin are easily prepared by in-situ polymerization on the surface of the reinforcing fiber. The thermoplastic resin is directly attached to the surface of the reinforcing fiber, and the composite material formed by the two can achieve higher interface peeling strength and mechanical properties.

[0005] Preferably, the weight average molecular weight of the thermoplastic resin is 60,000 or more.

[0006] Preferably, the general formula I is

[0007] Preferably, in the general formula I, Ar1 comprises the following structural units wherein R1 is selected from sulfonyl, hydrocarbon or optionally substituted hydrocarbon, R 1a , R 1b At least one independently selected from hydrogen and hydrocarbon groups.

[0008] Preferably, in the general formula I, Ar2 comprises at least one of the following structural units: In the above structural unit, R2 is selected from sulfonyl, hydrocarbon or optionally substituted hydrocarbon, R 2a , R 2b , R 3a , R 3b , R 4a , R 4b , R5 is independently selected from at least one of hydrogen and hydrocarbon group.

[0009] Preferably, the glass transition temperature of the thermoplastic resin is 90-110°C.

[0010] Preferably, the general formula I is specifically

[0011] When general formula I possesses this structural feature, the thermoplastic resin formed by this structure has better adhesion to the reinforcing fibers and mechanical properties.

[0012] Preferably, the degree of polymerization n of formula I is ≥150.

[0013] Preferably, the general structural formula of the thermoplastic resin is

[0014]

[0015] According to the second aspect of the present invention, a method for preparing the thermoplastic resin as described above is provided, comprising: allowing the monomer raw material to undergo a polymerization reaction under the action of a catalyst to generate a segment in accordance with the general formula I, the reaction temperature of the polymerization reaction being T, 100°C ≤ T < 180°C; the monomer raw material comprises a bisphenol glycidyl ether type epoxy resin and a dihydric phenol compound, Ar1 included in the segment in accordance with the general formula I is provided by the bisphenol glycidyl ether type epoxy resin, and Ar2 included in the segment in accordance with the general formula I is provided by the dihydric phenol compound; the catalyst comprises at least one of a quaternary amine catalyst, a phosphine catalyst, an organic phosphorus catalyst, a tertiary amine catalyst, and an imidazole catalyst. Under the catalytic action of the above catalyst, a thermoplastic resin having a segment in accordance with the general formula I can be successfully prepared under the above reaction conditions, the reaction conditions are mild, and the degree of reaction is highly controllable. Preferably, the reaction temperature of the polymerization reaction is T ≥ 150°C.

[0016] Preferably, the quaternary amine catalyst includes at least one of tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium hydroxide, triethylmethylammonium chloride, tetraethylammonium chloride, tetraethylammonium bromide, tetraethylammonium iodide, tetrapropylammonium bromide, tetrapropylammonium hydroxide, tetrabutylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium iodide, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylammonium hydroxide, benzyltributylammonium chloride, and phenyltrimethylammonium chloride.

[0017] Preferably, the phosphine catalyst includes at least one of triphenylphosphine, tri-o-tolylphosphine, tri(2,4-dimethylphenyl)phosphine, tri(2,5-dimethylphenyl)phosphine, tri(o-methoxyphenyl)phosphine, and dicyclohexylphenylphosphine.

[0018] Preferably, the organophosphorus catalyst includes at least one of tetramethyl phosphonium bromide, tetramethyl phosphonium iodide, tetramethyl phosphonium hydroxide, trimethylcyclohexyl phosphonium chloride, trimethylcyclohexyl phosphonium bromide, trimethylbenzyl phosphonium chloride, trimethylbenzyl phosphonium bromide, tetraphenyl phosphonium bromide, triphenylmethyl phosphonium bromide, triphenylmethyl phosphonium iodide, triphenylethyl phosphonium chloride, triphenylethyl phosphonium bromide, triphenylethyl phosphonium iodide, triphenylbenzyl phosphonium chloride, and triphenylbenzyl phosphonium bromide.

[0019] Preferably, the tertiary amine catalyst includes triethanolamine.

[0020] Preferably, the imidazole catalyst includes at least one of 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-undecylimidazole, 2-ethyl-4-methylimidazole and 1-cyanoethyl-2-methylimidazole.

[0021] Preferably, the catalyst comprises a quaternary ammonium catalyst, and the quaternary ammonium catalyst comprises tetrabutylammonium bromide.

[0022] Preferably, the amount of the catalyst is calculated by weight, W1 represents the amount of the catalyst, W0 represents the total amount of the bisphenol glycidyl ether epoxy resin and the dihydric phenol compound, W1 / W0=0.5% to 2%, and the catalyst is tetrabutylammonium bromide.

[0023] Preferably, W1 / W0=1-2%.

[0024] According to a third aspect of the present invention, there is provided a fiber-reinforced composite material, the fiber-reinforced composite material being composited with reinforcing fibers and the thermoplastic resin as described above. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a reaction mechanism diagram of treatment group 1A of Example 1;

[0026] Figure 2 This is a reaction mechanism diagram of the control group 1A of Example 1. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0028] Example 1

[0029] The raw materials used to prepare the thermoplastic resin in this embodiment are composed of reactive monomers and catalysts. Thermoplastic resins with different molecular structures can be prepared by selecting different types of reactive monomers and matching corresponding catalysts. Based on the different target molecular structures of the thermoplastic resins to be prepared, different treatment groups and control groups are set in this embodiment, wherein the treatment groups include treatment group 1A, treatment group 2A and treatment group 3A. The types of reactive monomers and catalysts used in the above treatment group and control group 1A are shown in Table 1.

[0030] Table 1. Types and ratios of reactive monomers used in the preparation of thermoplastic resins in each treatment group of this embodiment

[0031]

[0032] The methods for preparing thermoplastic resins for the treatment groups and the control group shown in Table 1 are as follows:

[0033] 1. Prepare the ingredients

[0034] (1) Reaction monomers: 100 g of reaction monomer I for different groups was weighed according to Table 1, and the specific amounts of reaction monomer II for different groups were as follows: the amounts of reaction monomer II for treatment groups 1A, 2A, and 3A were determined according to the ratio of epoxy groups contained in reaction monomer I to phenolic hydroxyl groups contained in reaction monomer II = 1:1; the amount of reaction monomer II for control group 1A satisfied that the ratio of the phenyl groups contained in reaction monomer I of control group 1A to the phenolic hydroxyl groups contained in reaction monomer II was equal to the ratio of the phenyl groups contained in reaction monomer I of treatment group 1A to the phenolic hydroxyl groups contained in reaction monomer II.

[0035] (2) Catalyst. The specific amounts of catalysts used in different groups are as follows: Treatment Group 1A, Treatment Group 2A, and Treatment Group 3A use tetrabutylammonium bromide as the catalyst, W1 represents the mass of tetrabutylammonium bromide, W0 represents the total mass of component A, and the amount of tetrabutylammonium bromide used satisfies W1 / W0=1%. Control Group 1A uses calcium hydrogen phosphate as the catalyst, and the mass of calcium hydrogen phosphate used is: the total mass of reaction monomer I and reaction monomer II weighed in Control Group 1A = 1%.

[0036] 2. Polymerization

[0037] The reaction monomer I and reaction monomer II used in each group are heated and mixed at 150°C to form a uniform mixture, and then the resulting mixture is cooled to 100°C, followed by adding a catalyst thereto, and finally the slurry is poured into a resin curing mold and cured at 150°C for 4 hours to obtain a molded thermoplastic resin.

[0038] Taking treatment group 1A as an example, the reaction mechanism of the in-situ polymerization involved in treatment group 1A is that under the catalytic action of the catalyst, the epoxy group of the bisphenol glycidyl ether type epoxy resin is ring-opened and undergoes polymerization reaction with the hydroxyl group of the dihydric phenol compound, thereby obtaining a product including a thermoplastic resin having a chain segment represented by general formula I in its molecular structure, wherein general formula I is The reaction mechanism is as follows Figure 1 The reaction mechanism of the in-situ polymerization involved in treatment group 2A and treatment group 3A is similar to that of treatment group 1A. The reaction mechanism of the in-situ polymerization involved in control group 1A is as follows Figure 2 The weight average molecular weight of the thermoplastic resins prepared in treatment group 1A, treatment group 2A, treatment group 3A and control group 1A of this embodiment all reached above 40,000.

[0039] Test Example 1

[0040] 1. Test subjects

[0041] The molded thermoplastic resins prepared in the treatment groups of Example 1 and the control group 1A were used as test objects.

[0042] 2. Test items and test standards

[0043] (1) Flexural strength: ASTM D790.

[0044] (2) Compression strength: ASTM D3140.

[0045] (3) Impact performance: GB / T 2571-1995.

[0046] 3. Test results

[0047] The test results of this test example are shown in Table 2. The molecular structures of the thermoplastic resins provided by treatment group 1A, treatment group 2A, and treatment group 3A of Example 1 all contain the following general chain segments: The above-mentioned general chain segment is marked as general formula I, and the molecular structure of the thermoplastic resin prepared by the control group 1A of Example 1 is referred to as Figure 2 As shown, the molecular structure of the thermoplastic resin does not have the segment structure shown in the above general formula I. From the test results, it can be seen that among the test objects, the comprehensive performance of the thermoplastic resin prepared by the control group 1A of Example 1 is significantly poor, which is specifically reflected in low bending strength, low compression strength, and low impact performance. This shows that the treatment groups 1A, 2A, and 3A of Example 1 introduce the segment structure shown in general formula I into the molecular structure of the thermoplastic resin, so that the thermoplastic resin has advantages in various aspects of bending strength, compression strength, and impact performance.

[0048] Table 2. Test results of test case 1

[0049] Thermoplastic resin group Bending strength / MPa Compression strength / MPa <![CDATA[Impact performance / (KJ / m 2 )]]> Example 1 Treatment Group 1A 110 90 40 Example 1 Treatment Group 2A 98 82 48 Example 1 Treatment Group 3A 118 98 32 Example 1 Control group 1A 50 42 8

[0050] Example 2

[0051] In this embodiment, the composite resin system used to prepare the thermoplastic resin is used to impregnate the reinforcing fibers, and then the composite resin system impregnated between the reinforcing fibers is triggered to undergo an in-situ polymerization reaction, thereby generating a thermoplastic resin on the surface of the reinforcing fibers, and the thermoplastic resin is directly compounded on the surface of the reinforcing fibers to obtain a reinforced fiber composite material. Among them, the composite resin system is composed of a reaction monomer and a catalyst. Thermoplastic resins with different molecular structures can be obtained by selecting different types of reaction monomers and matching corresponding catalysts. Based on the different target molecular structures for preparing thermoplastic resins, this embodiment follows the setting method of the treatment group and the control group in Example 1 for experimental design. The numbering of each group and the corresponding type of reaction monomer used are consistent with the contents shown in Table 1, and the preparation method of each group is also consistent with the corresponding group in Example 1. The raw materials required for each group are taken according to the above content. Specifically, the processing methods of treatment group 1A, treatment group 2A, and treatment group 3A in this embodiment are as follows:

[0052] S1. Preparation of composite resin system

[0053] S1.1 Preparation of Component A

[0054] Each treatment group corresponds to Table 1, and the reaction monomer I and reaction monomer II used are weighed according to the amount, and then the reaction monomer I used is heated to about 120°C, and then reaction monomer II is added thereto, and stirred thoroughly until the two are uniformly dissolved, thereby obtaining component A, and the temperature of component A is reduced to room temperature for use.

[0055] S1.2 Preparation of component B:

[0056] Tetrabutylammonium bromide is used as a catalyst, W1 represents the mass of tetrabutylammonium bromide, W0 represents the total mass of component A, the amount of tetrabutylammonium bromide used satisfies W1 / W0=1%, ​​methyl ethyl ketone (MEK) is used as a polar solvent, 40g of MEK is weighed, and then tetrabutylammonium bromide is added thereto, so that the above two catalysts are dissolved and fully dispersed in MEK to form a uniform solution, and component B is prepared for standby use. All treatment groups set in this embodiment prepare component B in the above manner.

[0057] S1.3 Mixing

[0058] Component A and component B are mixed, and the mixed slurry is stirred at a low speed first and then at a high speed until the mixture is uniformly mixed to obtain a prepreg containing a composite resin system.

[0059] S2. Preparation of reinforcing fiber prepreg

[0060] The prepreg liquid is passed into the impregnation tank, and the reinforcing fibers (the reinforcing fibers used in each treatment group of this embodiment are carbon fibers, and the manufacturer and product brand are Toray-T700) are pulled into the impregnation tank by a traction device to be impregnated with the prepreg liquid to obtain a prepreg semi-finished product, and the prepreg semi-finished product is heated to fully volatilize the MEK therein, thereby obtaining a reinforcing fiber prepreg. During the above impregnation process, the impregnation amount of the composite resin system is controlled to reach 40wt% of the reinforcing fiber prepreg by adjusting the tension of the traction device and the position of the roller, and the unit area weight of the reinforcing fibers in the reinforcing fiber prepreg is controlled to reach 170g / m 2 .

[0061] S3. Preparation of thermoplastic resin by in-situ polymerization

[0062] The reinforcing fiber prepreg is cut into a size of 20 cm×20 cm, heated to 150°C, and then hot-pressed at a pressure of 4 MPa, so that the composite resin system in the reinforcing fiber prepreg undergoes an in-situ polymerization reaction between the reinforcing fibers, thereby generating a thermoplastic resin on the surface of the reinforcing fibers, and the thermoplastic resin is directly compounded on the surface of the reinforcing fibers to obtain a reinforced fiber composite material. In this step, the weight average molecular weight of the obtained thermoplastic resin reaches more than 40,000 by specifically adjusting the hot pressing time of different groups (between 1 and 2 hours).

[0063] The treatment of control group 1A is as follows:

[0064] S1. Preparation of composite resin system

[0065] S1.1 Preparation of Component A

[0066] Corresponding to Table 1, the reaction monomer I and reaction monomer II are weighed according to the amount, and then the reaction monomer I is heated to about 120° C., and then reaction monomer II is added thereto, and stirred thoroughly until the two are uniformly dissolved, thereby obtaining component A, and the temperature of component A is reduced to room temperature for use.

[0067] S1.2 Preparation of component B:

[0068] Calcium hydrogen phosphate is used as a catalyst, and the mass of calcium hydrogen phosphate is 1% of the total mass of component A. Methyl ethyl ketone (MEK) is used as a polar solvent, 40g of MEK is weighed, and then calcium hydrogen phosphate and sodium tetraphenylborate are added thereto, so that the above two catalysts are dissolved and fully dispersed in MEK to form a uniform solution, thereby preparing component B for standby use.

[0069] S1.3 Mixing

[0070] Component A and component B are mixed, and the mixed slurry is stirred at a low speed first and then at a high speed until the mixture is uniformly mixed to obtain a prepreg containing a composite resin system.

[0071] S2. Preparation of reinforcing fiber prepreg

[0072] The prepreg prepared in the corresponding control group 1A was used to replace the prepreg used in the treatment group. Except for the above differences, other operations were performed according to S2 involved in the treatment group to complete the preparation of the reinforcing fiber prepreg of the control group 1A.

[0073] S3. Preparation of thermoplastic resin by in-situ polymerization

[0074] The reinforcing fiber prepreg prepared in the corresponding control group 1A was used to replace the reinforcing fiber prepreg used in the treatment group. Except for the above differences, other operations were carried out according to S3 involved in the treatment group to complete the preparation of the thermoplastic resin of the control group 1A, thereby preparing a reinforced fiber composite material.

[0075] Test Example 2

[0076] 1. Test subjects

[0077] The reinforced fiber composite material prepared in Example 2 was used as a test object.

[0078] 2. Test items and test standards

[0079] (1) Flexural strength: ASTM D7264-15 (composite materials three-point bending test).

[0080] (2) Interlaminar shear strength: ASTM D2344-16 (Interlaminar shear test for composite materials).

[0081] (3) Impact performance: ISO 179-1.

[0082] 3. Test results

[0083] The test results of this test example are shown in Table 3. As described above, the composite resin system used in the process of preparing the impregnated reinforcing fiber in Example 2 is the composite resin system for preparing the thermoplastic resin in Example 1, and in Example 2, the thermoplastic resin obtained by curing is directly compounded with the reinforcing fiber by a molding method, and according to the test results of this test example, the thermoplastic resin containing the segment structure shown in the above general formula I in the molecular structure has a better composite effect with the reinforcing fiber. In the reinforcing fiber-thermoplastic resin composite materials prepared by treatment group 1A, treatment group 2A, and treatment group 3A in Example 2, the thermoplastic resin can be tightly compounded with the reinforcing resin, so that the composite material has excellent flexibility and structural strength.

[0084] Table 3. Test results of test case 2

[0085]

[0086] Example 3

[0087] The treatment group 1A of Example 1 was used as a control to prepare a thermoplastic resin. The reaction temperature of the polymerization reaction in Example 1 was used to make the prepared thermoplastic resin have different weight average molecular weights. According to the different reaction temperatures adopted, treatment group 1B, treatment group 2B, treatment group 3B, treatment group 4B, and control group 1B were set. The reaction temperature, reaction time, and weight average molecular weight of the corresponding thermoplastic resin prepared in the polymerization reaction stage of each treatment group are specifically shown in Table 4. In the process of preparing the thermoplastic resin in each treatment group of this embodiment, except for the variables shown in Table 4, other materials and corresponding operations were consistent with those of treatment group 1A of Example 1.

[0088] Table 4. Reaction temperature corresponding to each treatment group in this example and weight average molecular weight of the obtained thermoplastic resin

[0089] Group Polymerization temperature and reaction time Weight average molecular weight of thermoplastic resin Example 1 Treatment Group 1A 150℃,4h 60000 Example 3 Treatment Group 1B 150℃,2h 40000 Example 3 Treatment Group 2B 150℃,6h 90000 Example 3 Control group 1B 120℃,4h 30000

[0090] Since the types of reaction monomers and catalysts used in the treatment groups and control groups of this embodiment are the same, the thermoplastic resins having molecular structures conforming to the following general formula can be obtained in each treatment group and control group.

[0091]

[0092] Test Example 3

[0093] 1. Test subjects

[0094] The thermoplastic resins prepared in treatment group 1A of Example 1 and each treatment group and control group of Example 3 were used as test objects.

[0095] 2. Test items and test standards

[0096] (1) Flexural strength: ASTM D790.

[0097] (2) Compression strength: ASTM D3140.

[0098] (3) Impact performance: GB / T 2571-1995.

[0099] 3. Test results

[0100] The test results of this test example are shown in Table 5. In Example 3, the weight average molecular weight of the thermoplastic resin to be prepared is controlled by changing the reaction temperature and reaction time of the polymerization reaction. The molecular weight of the thermoplastic resin prepared by the control group 1B of Example 3 is low, and the mechanical properties of the thermoplastic resin are significantly poorer than those of other thermoplastic resins. The thermoplastic resins prepared by the treatment group 1A of Example 1, the treatment group 1B of Example 3, and the treatment group 2B of Example 3 all reach a sufficiently high weight average molecular weight, so these thermoplastic resins all have excellent flexibility and mechanical strength, and, with the increase of the weight average molecular weight of the thermoplastic molecule, the comprehensive mechanical properties of the thermoplastic resin are further optimized.

[0101] Table 5. Test results of test case 3

[0102] Thermoplastic resin group Bending strength / MPa Compression strength / MPa <![CDATA[Impact performance / (KJ / m 2 )]]> Example 1 Treatment Group 1A 110 90 40 Example 3 Treatment Group 1B 100 82 32 Example 3 Treatment Group 2B 115 95 46 Example 3 Control group 1B 70 55 15

[0103] Example 4

[0104] This embodiment prepares a reinforced fiber composite material by referring to the method for preparing a reinforced fiber composite material applicable to treatment group 1A in embodiment 2, wherein the composite resin system used is the composite resin system used by treatment group 1A in embodiment 1 for preparing a thermoplastic resin.

[0105] The variable setting method of this embodiment is to use the treatment group 1A of Example 2 (hot pressing temperature 150°C, hot pressing time 1.5 hours) as a reference, and adjust the weight average molecular weight of the thermoplastic resin finally obtained by changing the heating temperature and hot pressing time involved in S3 in the preparation method of preparing thermoplastic resin by in-situ polymerization, and the weight average molecular weight of the thermoplastic resin obtained by the corresponding treatment group 1B of Example 3, the treatment group 2B of Example 3, and the control group 1B of Example 3 is experimentally designed. In addition to the above variables, the materials and other processing operations used in this embodiment for preparing the reinforced fiber composite material are strictly consistent with the method for preparing the reinforced fiber composite material for the treatment group 1A in Example 2. As shown in Table 6, the weight average molecular weights of the thermoplastic materials in the reinforced fiber composite material obtained in this embodiment, and the heating temperature and hot pressing time involved in S3 in the preparation method of preparing the corresponding in-situ polymerization for preparing the thermoplastic resin, in order to clearly show the differences between the experimental groups, the heating temperature and hot pressing time involved in S3 corresponding to the treatment group 1A of Example 2 are also loaded in Table 6.

[0106] Table 6. Reinforced fiber composite materials prepared in this example and their corresponding in-situ polymerization reaction conditions

[0107]

[0108]

[0109] Test Example 4

[0110] 1. Test subjects

[0111] The reinforced fiber composite material prepared in Example 4 was used as a test object.

[0112] 2. Test items and test standards

[0113] (1) Flexural strength: ASTM D7264-15 (composite materials three-point bending test).

[0114] (2) Interlaminar shear strength: ASTM D2344-16 (Interlaminar shear test for composite materials).

[0115] (3) Impact performance: ISO 179-1.

[0116] 3. Test results

[0117] The test results of this test example are shown in Table 7. In order to clearly show the differences between the experimental groups, the performance test results corresponding to the treatment group 1A of Example 2 are also included in Table 7. Based on the test results shown in Tables 6 and 7, when the weight average molecular weight of the thermoplastic resin obtained by in-situ polymerization reaches 40,000 or more, the mechanical strength of the reinforcing fiber-thermoplastic resin composite material obtained thereby is significantly improved. In general, as the weight average molecular weight of the thermoplastic resin increases, the interface bonding effect between the thermoplastic resin and the reinforcing fiber is better, and the mechanical strength of the corresponding reinforcing fiber-thermoplastic resin composite material is enhanced.

[0118] Table 7. Test results of test case 4

[0119]

[0120] Example 5

[0121] Thermoplastic resin was prepared by taking treatment group 1A of Example 1 as a control. In this embodiment, different treatment groups were set with the catalyst composition used to prepare thermoplastic resin as a variable. According to the different catalysts used, treatment group 1C, treatment group 2C, treatment group 3C, treatment group 4C, treatment group 5C, treatment group 1B, and treatment group 1D were set. The specific composition of the catalyst used in each treatment group is shown in Table 8, and the total mass of the catalyst used in each treatment group is controlled to be equal. In the process of preparing thermoplastic resin in each treatment group of this embodiment, except for the variables shown in Table 8, other materials and corresponding operations are consistent with treatment group 1A of Example 1, wherein the reaction temperature used in the polymerization reaction stage is 150°C and the reaction time is 4 hours.

[0122] Table 8. Catalyst compositions used in the preparation of thermoplastic resins in each treatment group of this example

[0123] Group Types of catalysts and corresponding feed amounts Example 1 Treatment Group 1A <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 1%]]> Example 5 Treatment Group 1B <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 0.5%]]> Example 5 Treatment Group 1C <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 1.5%]]> Example 5 Treatment Group 1D <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 2%]]> Example 5 Treatment Group 2C <![CDATA[Triphenylphosphine, W1 / W0 = 1%]]> Example 5 Treatment Group 3C <![CDATA[Triethanolamine, W1 / W0 = 1%]]> Example 5 Treatment Group 4C <![CDATA[Triphenylbenzylphosphonium chloride, W1 / W0 = 1%]]> Example 5 Treatment Group 5C <![CDATA[2-Methylimidazole, W1 / W0 = 1%]]>

[0124] Test Example 5

[0125] 1. Test subjects

[0126] The thermoplastic resins prepared in each treatment group of Example 5 were used as test objects.

[0127] 2. Test items and test standards

[0128] (1) Flexural strength: ASTM D790.

[0129] (2) Compression strength: ASTM D3140.

[0130] (3) Impact performance: GB / T 2571-1995.

[0131] 3. Test results

[0132] The test results of this test example are shown in Table 9. From the content shown in Table 8, it can be seen that the types of catalysts used to prepare thermoplastic resins in the treatment groups involved in Table 8 are different. Combined with the test results of this test example, it can be seen that the mechanical properties of the thermoplastic resins proposed in this scheme will be affected by the types of catalysts used in the preparation process. Under the same catalyst dosage, the mechanical properties of the thermoplastic resin prepared using tetrabutylammonium bromide as a catalyst are better. Based on the use of tetrabutylammonium bromide as a catalyst, it is found by adjusting the feeding amount of tetrabutylammonium bromide that when the feeding amount of tetrabutylammonium bromide satisfies W1 / W0=1%, ​​the mechanical properties of the thermoplastic resin prepared thereby are the best.

[0133] Table 9. Test results of test case 5

[0134] Group Bending strength / MPa Compression strength / MPa <![CDATA[Impact performance / (KJ / m 2 )]]> Example 1 Treatment Group 1A 110 90 40 Example 5 Treatment Group 1B 88 71 26 Example 5 Treatment Group 1C 105 82 34 Example 5 Treatment Group 1D 101 78 29 Example 5 Treatment Group 2C 98 75 28 Example 5 Treatment Group 3C 80 65 20 Example 5 Treatment Group 4C 73 55 24 Example 5 Treatment Group 5C 82 61 22

[0135] Example 6

[0136] In this example, a reinforced fiber composite material was prepared by referring to the method for preparing a reinforced fiber composite material applicable to treatment group 1A in Example 2.

[0137] This embodiment corresponds to Example 5, and the variable setting method is to change the catalyst composition of the composite resin system based on the composite resin system used in the treatment group 1A of Example 1, and the corresponding treatment group 1B of Example 5, the treatment group 1C of Example 5, the treatment group 1D of Example 5, the treatment group 2C of Example 5, the treatment group 3C of Example 5, the treatment group 4C of Example 5, and the treatment group 5C of Example 5 are experimentally designed. In addition to the above variables, the materials and other processing operations used in this embodiment for preparing the reinforced fiber composite material are strictly consistent with the method for preparing the reinforced fiber composite material applicable to the treatment group 1A (hot pressing time is 1.5 hours) in Example 2. As shown in Table 10, the reinforced fiber composite material obtained in this embodiment corresponds to the catalyst composition contained in the composite resin system used to prepare it. In order to clearly show the differences between the experimental groups, the catalyst type and corresponding amount used in the treatment group 1A of Example 2 are also loaded in Table 10.

[0138] Table 10. Composition of the reinforced fiber composite material prepared in this example and the corresponding catalyst used

[0139] Reinforced fiber-thermoplastic resin composite material group Types of catalysts and corresponding feed amounts Example 2 Treatment Group 1A <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 1%]]> Example 6 Treatment Group 1B <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 0.5%]]> Example 6 Treatment Group 1C <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 1.5%]]> Example 6 Treatment Group 1D <![CDATA[Tetrabutylammonium bromide, W1 / W0 = 2%]]> Example 6 Treatment Group 2C <![CDATA[Triphenylphosphine, W1 / W0 = 1%]]> Example 6 Treatment Group 3C <![CDATA[Triethanolamine, W1 / W0 = 1%]]> Example 6 Treatment Group 4C <![CDATA[Triphenylbenzylphosphonium chloride, W1 / W0 = 1%]]> Example 6 Treatment Group 5C <![CDATA[2-Methylimidazole, W1 / W0 = 1%]]>

[0140] Test Example 6

[0141] 1. Test subjects

[0142] The reinforced fiber composite material prepared in Example 6 was used as a test object.

[0143] 2. Test items and test standards

[0144] (1) Flexural strength: ASTM D7264-15 (composite materials three-point bending test).

[0145] (2) Interlaminar shear strength: ASTM D2344-16 (Interlaminar shear test for composite materials).

[0146] (3) Impact performance: ISO 179-1.

[0147] 3. Test results

[0148] The test results of this test example are shown in Table 11. In order to clearly show the differences between the experimental groups, the performance test results corresponding to the treatment group 1A of Example 2 are also included in Table 11. It can be seen from the test results that the use of the catalyst involved in the preparation of the thermoplastic resin will also affect the mechanical properties of the reinforcing fiber-thermoplastic resin composite material composed of the thermoplastic resin and the reinforcing fiber. The test results show that based on the mechanical properties of the reinforcing fiber-thermoplastic resin composite material, the preferred catalyst type is tetrabutylammonium bromide.

[0149] Table 11. Test results of test case 4

[0150]

[0151]

[0152] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. A thermoplastic resin, characterized in that: The molecular structure of the thermoplastic resin contains the chain segments shown in the following general formula I, wherein the general formula I is In the general formula I, Ar1 and Ar2 are independently selected from aromatic groups containing a benzene ring, R is a hydrocarbon group, and n is the degree of polymerization of the chain segment represented by the general formula I; The weight average molecular weight of the thermoplastic resin is greater than 40,000, and the glass transition temperature of the thermoplastic resin is 85 to 130°C.

2. The thermoplastic resin according to claim 1, characterized in that: In the general formula I, Ar1 includes the following structural units wherein R1 is selected from sulfonyl, hydrocarbon or optionally substituted hydrocarbon, R 1a , R 1b At least one independently selected from hydrogen and hydrocarbon groups.

3. The thermoplastic resin according to claim 1, characterized in that In the general formula I, Ar2 comprises at least one of the following structural units: In the above structural unit, R2 is selected from sulfonyl, hydrocarbon or optionally substituted hydrocarbon, R 2a , R 2b , R 3a , R 3b , R 4a , R 4b , R5 is independently selected from at least one of hydrogen and hydrocarbon group.

4. The thermoplastic resin according to claim 1, characterized in that: The glass transition temperature of the thermoplastic resin is 90 to 110°C.

5. The thermoplastic resin according to any one of claims 1 to 4, characterized in that: The general formula I is specifically 6. The thermoplastic resin according to claim 5, characterized in that: The degree of polymerization n of the chain segment represented by the general formula I is ≥150.

7. A method for preparing a thermoplastic resin according to any one of claims 1 to 6, characterized in that: include: The monomer raw material is polymerized under the action of a catalyst to generate a chain segment in accordance with the general formula I, wherein the reaction temperature of the polymerization reaction is T, 100°C≤T<180°C; The monomer raw material includes a bisphenol glycidyl ether type epoxy resin and a dihydric phenol compound, Ar1 included in the chain segment shown in the general formula I is provided by the bisphenol glycidyl ether type epoxy resin, and Ar2 included in the chain segment shown in the general formula I is provided by the dihydric phenol compound; The catalyst includes at least one of a quaternary amine catalyst, a phosphine catalyst, an organic phosphorus catalyst, a tertiary amine catalyst, and an imidazole catalyst.

8. The method for preparing a thermoplastic resin according to claim 7, characterized in that: The catalyst includes the quaternary ammonium catalyst, and the quaternary ammonium catalyst includes tetrabutylammonium bromide.

9. The method for preparing a thermoplastic resin according to claim 8, characterized in that: According to the calculation based on the feed weight, W1 represents the feed amount of the catalyst, W0 represents the total feed amount of the bisphenol glycidyl ether epoxy resin and the dihydric phenol compound, and W1 / W0=0.5% to 2%.