High-strength, high-transparency and high-haze cellulose membrane and manufacturing method thereof
By hot-pressing and double-rolling calendering of paper materials with high cellulose content, the problems of complex preparation process and insufficient mechanical properties of high-transparency and high haze cellulose films in the prior art are solved, and high strength, High transparency and haze cellulose membrane, suitable for electronics.
Patent Information
- Application Number
- CN202310511999.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, when preparing high-transparency and high-haze cellulose films, the process is complex, the energy consumption is large or the mechanical properties are weak, making it difficult to achieve simple and easy to produce on a large scale.
The paper material with a cellulose content >90% is used to perform hot-pressing and double-rolling calendering after simple soaking of ionic liquid. The solid content of the cellulose/solvent gel and the roughness of the calendering roller are controlled, and the light transmittance of the film is adjusted. Haze, obtain high strength, high transparency and haze cellulose films.
Achieve high light transmittance >80%, high haze >50%, tensile strength >250MPa, elongation at break >10%, and optimize cellulose optical and mechanical properties through calendering ratio and roll roughness adjustment, providing New application ideas for cellulose optical devices.
Smart Images

Figure CN118909276A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cellulose film preparation, and in particular relates to a high-strength, high-transparency and high-haze cellulose film and a manufacturing method thereof. Background Art
[0002] With the depletion of fossil energy and increasingly prominent environmental problems, the application of biodegradable and renewable materials in the field of electronic devices has attracted extensive research attention. Cellulose film has the advantages of excellent mechanical properties, light weight, high transparency, good flexibility, renewable, biodegradable and low price. Its application in flexible solar cell substrate materials, organic light-emitting diodes (OLEDs), touch screens, etc. is favored by researchers. Compared with high-transparency and low-haze cellulose film substrates, in addition to providing mechanical support for devices, high-transparency and high-haze cellulose films can also serve as light management layers, which can improve the performance of devices by reasonably coupling light into or out of optoelectronic devices under wide wavelengths and wide incident angles. Therefore, the development of high-transmittance and high-haze cellulose films is crucial for their application in optoelectronic devices and improving the performance of optoelectronic devices.
[0003] At present, there are two main ways to prepare high-transmittance and high-haze materials: (1) Add scattering particles to the transparent matrix to reflect, refract and scatter light between different materials, thereby producing a light diffusion effect, thereby achieving high haze; (2) Introduce microstructures on the surface of transparent matrix materials, and use the surface microstructures to refract and scatter light on the surface of the material, thereby achieving high haze. Therefore, the design and research of high-transmittance and high-haze cellulose membranes also focus on these two methods. Li et al. achieved the adjustment of the haze of nanocellulose membranes by controlling the aspect ratio of nanocellulose and the composite of nanocelluloses with different aspect ratios. The transmittance and haze of the nanocellulose membranes finally obtained were as high as 89% and 77%, respectively (Cellulose, 2019, 27: 1315-1326). After Chen et al. silanized the surface of the CNF membrane, the CNF membrane not only achieved light management (transmittance: 90.2%, haze: 46.5%) but also had a self-cleaning function (contact angle of 159.6°). Using it in solar cells can improve the overall performance by 10.43% (ACS Sustainable Chemistry & Engineering, 2018, 6: 5173-5181). Cheng et al. introduced scattering particles chitosan particles into the cellulose / AmimCl solution. By controlling the size and content of chitosan particles, the transmittance and haze of the cellulose / chitosan blended membrane can be as high as 85% and 93%, respectively (Advanced Materials Technologies, 2020: 2000378-2000385). Usually, after the introduction of scattering particles, due to the poor compatibility between the scattering particles and the matrix and the presence of the phase interface, the mechanical strength of the blended membrane will inevitably drop sharply. Hu et al. finally obtained a full cellulose membrane by impregnating cellulose paper as a scatterer with a transparent sodium carboxymethyl cellulose (CMC-Na) solution. When the mass ratio of CMC-Na to northern wood fiber was 7:3, its transmittance was as high as 90%, the haze was as high as 82%, and the tensile strength was as high as 140 MPa (ACS Sustainable Chemistry & Engineering, 2018, 6: 6974-6980).
[0004] Although great progress has been made in the research of high transmittance and high haze cellulose membranes, the current methods are either complicated, energy-intensive, and cause certain environmental pollution, or have weak mechanical properties and are difficult to achieve continuous production. Therefore, it is still a huge challenge to prepare cellulose membranes with high transmittance, high haze, and excellent mechanical properties in a simple and easy-to-scale production method. Summary of the invention
[0005] In order to solve the above problems, the present invention proposes a cellulose film with high strength, high transparency and high haze and a method for manufacturing the same. Various papers with a cellulose content of >90% are used as raw materials. After simple soaking in ionic liquid and then hot pressing and double-roll calendering, a cellulose film with high strength, high transparency and high haze can be obtained.
[0006] In order to achieve the above object, the present invention provides a method for manufacturing a cellulose film with high strength, high transparency and high haze, comprising the following steps:
[0007] Step 1: Soaking the cellulose raw material in solvent A, so that the cellulose raw material absorbs solvent A;
[0008] Step 2: hot pressing the cellulose soaked in solvent A in step 1 to obtain a cellulose / solvent A gel with fluidity;
[0009] Step 3: repeatedly washing the cellulose / solvent A gel with solvent B to regenerate it, while removing solvent A to obtain a cellulose hydrogel;
[0010] Step 4: calendering the cellulose hydrogel through a double-roll calender and drying to obtain a cellulose film;
[0011] In one embodiment of the present invention, the solid content of cellulose in the cellulose / solvent A gel is 15-40 wt %, preferably 25-36.2 wt %, for example, 25 wt %, 30 wt %, 35 wt %, 36.2 wt %.
[0012] In one embodiment of the present invention, at least one of the pair of calendering rolls of the twin-roll calender is a calendering roll having roughness.
[0013] Preferably, the roughness of the calendering roller is 100 to 10000 meshes; more preferably, it is 120 to 2000 meshes.
[0014] For example, 120 mesh, 200 mesh, 400 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1600 mesh, 1800 mesh, 2000 mesh or any range between any two of the above points or any point within the range.
[0015] Preferably, the pressure between the rolls is 0.01 MPa-5 MPa, more preferably 0.05 MPa-3 MPa, and further preferably 0.5-1.5 MPa.
[0016] In one embodiment of the present invention, the gap between the two rollers is controlled to be 0-1 mm, preferably 0.01-0.5 mm, and the gap between the two rollers is controlled to obtain a cellulose film with a calendering multiple ≥ 1.5; preferably the calendering multiple is 2; wherein the calendering multiple R is calculated by the following formula: R = l / l0, l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0017] In one embodiment of the present invention, the solvent A is one or more of an ionic liquid, a mixed solvent formed by an ionic liquid and an organic solvent, an amine oxide system, a carbamate system, an alkaline solution, an alkali / urea aqueous solution, an alkali / thiourea aqueous solution, and an acid solution.
[0018] Preferably, the ionic liquid is a molten salt formed by substituted or unsubstituted imidazolium or pyridinium cations and anions and having a melting point below 100°C.
[0019] Preferably, the substituent on the imidazole or pyridinium cation is C 1-6 Alkyl, C 1-6 The anion is one or more of an alkyl acid ion, a halide ion, and an organic phosphate ion.
[0020] For example, the ionic liquid is selected from one or more of 1-allyl-3-methylimidazolium chloride solution (AmimCl), 1-butyl-3-methylimidazolium acetate solution (BmimAc) ionic liquid and 1-ethyl-3-methylimidazolium acetate solution (EmimAc).
[0021] In one embodiment of the present invention, the organic solvent is selected from one or more of N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, acetone, tetrahydrofuran, pyridine, chloroform, dichloromethane and alcohols.
[0022] In one embodiment of the present invention, the alcohols are exemplified by ethanol, methanol and isopropanol.
[0023] In one embodiment of the present invention, the mixed solvent formed by the ionic liquid and the organic solvent may be, for example, N,N-dimethylacetamide / lithium chloride (DMAc / LiCl) or liquid ammonia / NH4SCN;
[0024] In one embodiment of the present invention, the amine oxide system is N-methylmorpholine oxide.
[0025] In one embodiment of the present invention, the alkaline solution is an aqueous sodium hydroxide solution and / or an aqueous potassium hydroxide solution.
[0026] In one embodiment of the present invention, the acid solution is selected from one or more of a phosphoric acid solution, a sulfuric acid solution, and an acetic acid solution.
[0027] In one embodiment of the present invention, the solvent B in step 3 is selected from one or more of water, ethanol, ionic liquid / water, and ionic liquid / ethanol.
[0028] Optionally, in the ionic liquid / water or ionic liquid / ethanol, the content of the ionic liquid is 5 wt% to 80 wt%.
[0029] In one embodiment of the present invention, before step 1, a step of placing the cellulose raw material in an oven for drying is also included.
[0030] Preferably, the temperature of the solvent A is 100-120° C., and the soaking time is 5 s to 90 s.
[0031] For example, the filter paper is placed in a vacuum oven at 80° C. to dry for 48 hours, and then the filter paper is immersed in an ionic liquid 1-ethyl-3-methylimidazolium acetate (EmimAc) solution at 110° C. for 30 seconds.
[0032] In one embodiment of the present invention, in step 2, the cellulose soaked with solvent A is sequentially laid on a mold frame for hot pressing, and the hot pressing conditions are: pressing at a pressure of 8.0-8.5 MPa for 40-80 min in a vacuum laminator at 100-120°C.
[0033] For example, three layers of filter paper soaked with ionic liquid were sequentially laid on a 1 mm thick mold frame, and then pressed at a pressure of 8.2 MPa for 60 min in a vacuum laminator at 110°C.
[0034] In one embodiment of the present invention, the cellulose is selected from one or more of microcrystalline cellulose, pulp, paper, plant straw, grass plants, Chinese medicine residues, waste wood chips, bagasse, reeds, corn cobs, fruit shells, plant stems and leaves, wood powder, sawdust and bamboo.
[0035] In one embodiment of the present invention, the pulp is selected from one or more of cotton pulp, wood pulp, bamboo pulp and straw pulp.
[0036] In one embodiment of the present invention, the cellulose content of the paper is greater than 90%, for example, the paper is selected from one or more of qualitative filter paper, absorbent paper, toilet paper and A4 printing paper.
[0037] In one embodiment of the present invention, the plant straw is selected from one or more of wheat straw, corn straw, cotton straw, soybean straw, sorghum straw and rice straw.
[0038] In one embodiment of the present invention, the grass plant is selected from one or more of foxtail grass, pennisetum, and barnyard grass.
[0039] The present invention also provides a high-strength, high-transparency and high-haze cellulose film, which is prepared by the above-mentioned method for manufacturing the high-strength, high-transparency and high-haze cellulose film.
[0040] In one embodiment of the present invention, the cellulose film has a light transmittance of >80%, a haze of >50%, a tensile strength of >250 MPa, and an elongation at break of >10%.
[0041] In one embodiment of the present invention, the cellulose film material with high strength, high transparency and high haze is widely used in electronic fields such as OLED lighting and display, solar panels, etc.
[0042] Beneficial effects of the present invention:
[0043] In the process of preparing cellulose film, the present invention controls the cellulose solid content in the cellulose / solvent A gel to be ≥25wt%, so that the solid content is kept high, the hydrogen bond density is high during coagulation-regeneration, and the roughness of the calendering roller is selectively adjusted, thereby adjusting the surface roughness of the film, improving its light transmittance and haze, and giving the film surface microstructure through double-roll calendering, so that the film surface is smooth, resulting in good mechanical properties of the final film and high haze. The light transmittance of the obtained film is greater than 80%, the haze is greater than 50%, the tensile strength is greater than 250MPa, the elongation at break is greater than 10%, and the optical and mechanical properties of the cellulose film can be adjusted by the calendering ratio and the roughness of the calendering roller, providing a new idea for regulating the light transmittance and haze of cellulose optical devices.
[0044] The present invention uses environmentally friendly, renewable and degradable cellulose as raw material, and after simple soaking in solvent and then hot pressing and double-roll calendering, a cellulose film with high strength, high transparency and high haze can be produced, which solves the problems of existing petroleum-based materials such as high pollution and non-degradability. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 Digital photos of the prepared cellulose films with different haze at different heights from the background (a) 0 mm, (b) 3 mm, and (c) 10 mm;
[0046] Figure 2 This is a surface morphology image of the smooth surface cellulose film prepared in Example 1;
[0047] Figure 3 This is a surface morphology image of the rough surface cellulose membrane prepared in Example 1. DETAILED DESCRIPTION
[0048] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0049] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0050] Example 1
[0051] First, the filter paper was dried in a vacuum oven at 80°C for 48 hours; then, the filter paper was immersed in an ionic liquid 1-ethyl-3-methylimidazolium acetate (EmimAc) solution at 110°C for 30 seconds, and three layers of filter paper soaked in ionic liquid were laid in a 1mm thick mold frame in sequence, and then pressed in a vacuum laminator at 110°C at a pressure of 8.2MPa for 60 minutes to obtain a cellulose / EmimAc ion gel, wherein the solid content of cellulose was 35wt%.
[0052] The obtained cellulose / EmimAc ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0053] During the calendering process, the roughness of one roller of the calendering pair of rollers was controlled to be 400 mesh, the other roller was a smooth roller, the pressure between the rollers was 0.5 MPa, and the gap between the two rollers was controlled to be 0.1 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0054] Example 2
[0055] First, the absorbent paper was placed in a vacuum oven at 80°C and dried for 24 hours; then, the filter paper was immersed in the ionic liquid EmimAc at 110°C for 30 seconds, and three layers of filter paper soaked in the ionic liquid were laid in turn on a 1 mm thick mold frame, and then pressed at a pressure of 8.2 MPa in a vacuum laminator at 110°C for 60 minutes to obtain cellulose / EmimAc ion gel with a cellulose solid content of 35 wt%.
[0056] The obtained cellulose / EmimAc ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0057] During the calendering process, the roughness of both rollers of the calendering pair of rollers was controlled to be 120 mesh, the pressure between the rollers was 1 MPa, and the gap between the two rollers was controlled to be 0.01 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0058] Example 3
[0059] First, the filter paper was dried in a vacuum oven at 80°C for 48 hours; then, the filter paper was immersed in the ionic liquid BmimAc at 110°C for 30 seconds, and three layers of filter paper soaked in the ionic liquid were laid in turn on a 1 mm thick mold frame; then, it was pressed in a vacuum laminator at 110°C at a pressure of 8.2 MPa for 60 minutes to obtain a cellulose / BmimAc ion gel with a cellulose solid content of 40 wt%.
[0060] The obtained cellulose / BmimAc ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0061] During the calendering process, the roughness of both rollers of the calendering pair of rollers was controlled to be 400 mesh, the pressure between the rollers was 1.5 MPa, and the gap between the two rollers was controlled to be 0.5 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0062] Example 4
[0063] First, toilet paper was placed in a vacuum oven at 80°C and dried for 48 hours. Subsequently, the filter paper was immersed in the ionic liquid BmimCl at 110°C for 30 seconds. Ten layers of filter paper soaked in the ionic liquid were laid in a 1 mm thick mold frame in turn, and then pressed at a pressure of 5 MPa for 60 minutes in a vacuum laminator at 110°C. A cellulose / EmimAc ion gel was obtained, and the solid content of cellulose was 25 wt%.
[0064] The obtained cellulose / BmimCl ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0065] During the calendering process, the roughness of one roller of the calendering pair of rollers was controlled to be 400 mesh, the other roller was a smooth roller, the pressure between the rollers was 1.5 MPa, and the gap between the two rollers was controlled to be 0.2 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0066] Example 5
[0067] First, the absorbent paper was placed in a vacuum oven at 90°C and dried for 24 hours; then, the filter paper was immersed in the ionic liquid EmimAc at 90°C for 30 seconds, and three layers of filter paper soaked in the ionic liquid were laid in turn on a 1 mm thick mold frame; then, it was pressed in a vacuum laminator at 110°C at a pressure of 12 MPa for 50 minutes; and a cellulose / EmimAc ion gel was obtained, with a cellulose solid content of 35 wt%.
[0068] The obtained cellulose / EmimAc ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0069] During the calendering process, the roughness of both rollers of the calendering pair of rollers was controlled to be 1000 mesh, the pressure between the rollers was 2 MPa, and the gap between the two rollers was controlled to be 0.05 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0070] Example 6
[0071] First, toilet paper was dried in a vacuum oven at 80°C for 24 hours. Subsequently, the filter paper was immersed in the ionic liquid EmimAc at 60°C for 10 seconds, and 10 layers of filter paper soaked in the ionic liquid were laid in sequence on a 1 mm thick mold frame. The filter paper was then pressed at a pressure of 8.2 MPa at 110°C in a vacuum laminator for 60 minutes to obtain a cellulose / EmimAc ion gel with a cellulose solid content of 15 wt%.
[0072] The obtained cellulose / EmimAc ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0073] During the calendering process, the roughness of both rollers of the calendering pair of rollers was controlled to be 1200 mesh, the pressure between the rollers was 0.5 MPa, and the gap between the two rollers was controlled to be 0.01 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0074] Example 7
[0075] First, the absorbent paper was placed in a vacuum oven at 90°C and dried for 48 hours. Subsequently, the filter paper was immersed in the ionic liquid BmimCl at 100°C for 20 seconds, and three layers of filter paper soaked in the ionic liquid were laid in turn on a 1 mm thick mold frame. The cellulose / EmimAc ion gel was obtained by pressing at a pressure of 5 MPa at 100°C for 40 minutes in a vacuum laminator. The solid content of cellulose was 35 wt%.
[0076] The obtained cellulose / BmimCl ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0077] During the calendering process, the roughness of one roll of the calendering pair of rollers was controlled to be 2000 mesh, the other roll was a smooth roll, the pressure between the rolls was 2 MPa, and the gap between the two rolls was controlled to be 0.03 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0078] Example 8
[0079] First, the filter paper was dried in a vacuum oven at 80°C for 48 hours; then, the filter paper was immersed in the ionic liquid EmimAc at 110°C for 30 seconds, and three layers of filter paper soaked in the ionic liquid were laid in turn on a 1 mm thick mold frame; then, it was pressed in a vacuum laminator at 110°C at a pressure of 8.2 MPa for 60 minutes; and a cellulose / BmimAc ion gel was obtained, with a cellulose solid content of 36.2 wt%.
[0080] The obtained cellulose / EmimAc ion gel was repeatedly washed with deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0081] During the calendering process, the roughness of both rollers of the calendering pair of rollers was controlled to be 2000 mesh, the pressure between the rollers was 1 MPa, and the gap between the two rollers was controlled to be 0.15 mm, so as to obtain a cellulose film with a calendering multiple of 2. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0082] Example 9
[0083] First, the filter paper was dried in a vacuum oven at 80°C for 48 hours, and then immersed in the ionic liquid 1-ethyl-3-methylimidazolium acetate (EmimAc) at 110°C for 30 seconds. Three layers of filter paper soaked in the ionic liquid were laid in a 1 mm thick mold frame in turn; then pressed at a pressure of 8.2 MPa in a vacuum laminator at 110°C for 60 minutes; and a cellulose / EmimAc ion gel was obtained with a cellulose solid content of 36.2 wt%.
[0084] The obtained cellulose / EmimAc ion gel was repeatedly washed with 20° C. deionized water to remove the ionic liquid, thereby obtaining a cellulose hydrogel. Finally, the cellulose hydrogel was calendered by a double-roll calender and dried to obtain a cellulose membrane.
[0085] During the calendering process, the cellulose film was passed through smooth calendering rollers, the pressure between the rollers was 0.5 MPa, and the gap between the two rollers was controlled to be 0.2 mm, and a cellulose film with a calendering multiple of 2 was obtained. The calendering multiple (R) was calculated by the following formula: R = l / l0, where l is the length of the cellulose film after calendering, and l0 is the length of the cellulose hydrogel before calendering.
[0086] Comparative Example 1
[0087] Wood pulp was selected as the raw material, 95 g of 1-ethyl-3-methylimidazolium acetate (EmimAc) ionic liquid was weighed, 5 g of dry wood pulp was added, and stirred and dissolved at 80°C. After 60 minutes, a uniform transparent solution was formed (the solid content of wood pulp in the wood pulp / EmimAc solution was 5 wt%). 20°C water was used as a coagulation bath to obtain cellulose hydrogel, which was then washed with water and dried at 60°C to obtain a membrane material.
[0088] Figure 1Digital photos of different haze cellulose films prepared at different heights from the background: 0 mm, 3 mm, and 10 mm; To more intuitively show that the cellulose film has high light transmittance and high haze, digital photos of three samples, a (the sample prepared in Example 9), b (the sample prepared in Example 1), and c (the sample prepared in Example 3), at heights of 0 mm, 3 mm, and 10 mm from the background are taken. When the three samples a, b, and c are 0 mm from the background, since all three samples have a very high light transmittance, the background numbers can be clearly seen through the three samples; when the three samples a, b, and c are 3 mm from the background, due to the haze a < b < c, the degree of blurring of the background numbers is a < b < c; however, when the distance of the three samples a, b, and c from the background increases to 10 mm, only a can clearly see the background numbers, while b and c cannot be seen clearly due to the high haze causing the background numbers to be blurred.
[0089] Figure 2 Figure shows the surface morphology of the smooth cellulose film obtained by the smooth calendering roll in Example 1. When the calendering roll is smooth, the surface of the cellulose film obtained by calendering has relatively small undulations and a relatively small surface roughness (about 5 μm), thus proving that its surface is flat and smooth.
[0090] Figure 3 Figure shows the surface morphology of the rough cellulose film obtained by the rough calendering roll in Example 1. It can be seen that the surface has relatively large undulations and a relatively large surface roughness (>36 μm), thus showing a surface with a rough and uneven microstructure.
[0091] The light transmittance and haze of the cellulose films prepared in Examples 1 - 9 and Comparative Example 1 between wavelengths of 400 - 800 nm were measured using a UV spectrophotometer Perkin-Elmer Lambda 950. The mechanical properties were tested at room temperature using a universal testing machine Instron 3365 with a gauge length of 20 mm and a tensile speed of 2 mm / min.
[0092] The test results are shown in Table 1 (the light transmittance and haze values in Table 1 are the measured values corresponding to a wavelength of 700 nm using the UV spectrophotometer).
[0093] Table 1. Physical properties of cellulose films
[0094]
[0095] As can be seen from Table 1, due to the low cellulose solid content in Comparative Example 1, the hydrogen bond density is low during coagulation-regeneration, and the film surface is smooth, resulting in poor mechanical properties and low haze of the final film. Although the cellulose solid content in Comparative Example 9 is high and the hydrogen bond density is high during coagulation-regeneration, due to the smooth film surface, the final film has good mechanical properties but still has low haze.
[0096] The solid content of cellulose in Examples 1-8 is high, the hydrogen bond density is high during coagulation-regeneration, and the film surface is given a microstructure after double-roll calendering, making the film surface smooth, resulting in good mechanical properties of the final film and high haze. The cellulose solid content in the embodiment of the present invention is the highest (≥15wt%), and the cellulose molecular chains are entangled with each other to form a denser hydrogen bond cross-linked network structure, so that it exhibits a tougher state than conventional cellulose hydrogels, and the tensile strength and elongation at break of the obtained cellulose hydrogel film are as high as 9.1MPa and 252%, respectively.
[0097] Compared with the cellulose hydrogel obtained by the traditional solution method, the cellulose solid content is low (<10wt%), the entanglement between the cellulose chains in the hydrogel is weak, and the physical cross-linking network formed by the cellulose hydrogen bonds is less, so that the traditional cellulose hydrogel exhibits weak tensile strength (2.2MPa) and low elongation at break (65%). The cellulose hydrogel obtained in the embodiment of the present invention has a very high elongation at break, indicating that the hydrogel has good ductility, so that a high-strength and high-haze cellulose film material can be prepared by calendering.
[0098] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for producing a high-strength, high-transparency and high-haze cellulose film, It is characterized in that The steps include: Step 1: Soaking the cellulose raw material in solvent A, so that the cellulose raw material absorbs solvent A; Step 2: hot pressing the cellulose soaked in solvent A in step 1 to obtain a cellulose / solvent A gel with fluidity; Step 3: repeatedly washing the cellulose / ionic liquid gel with solvent B to regenerate it, while removing solvent A to obtain a cellulose hydrogel; Step 4: calendering the cellulose hydrogel through a double-roll calender and drying to obtain a cellulose film; Wherein, the cellulose solid content in the cellulose / solvent A gel is ≥25wt%.
2. The manufacturing method according to claim 1, It is characterized in that The cellulose content in the cellulose / solvent A gel is 15 wt% to 40 wt%, preferably 25 to 36.2 wt%, for example, 25 wt%, 30 wt%, 35 wt%, 36.2 wt%.
3. The manufacturing method according to claim 1, It is characterized in that At least one of the pair of calendering rolls of the twin-roll calender is a calendering roll having roughness. Preferably, the roughness of the calendering roller is 100-10000 mesh; more preferably, it is 120-2000 mesh, for example, 120 mesh, 200 mesh, 400 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1600 mesh, 1800 mesh, 2000 mesh or any range between any two of the above values or any point within the range. Preferably, the pressure between the rolls is 0.01 MPa-5 MPa, more preferably 0.05 MPa-3 MPa, and further preferably 0.5-1.5 MPa. Preferably, the gap between the two rollers is controlled to be 0-1 mm, preferably 0.01-0.5 mm, to obtain a cellulose film with a calendering multiple ≥ 1.5, for example, a calendering multiple of 2; wherein the calendering multiple R is calculated by the following formula: R = l / l 0 , l is the length of the cellulose film after calendering, l 0 is the length of cellulose hydrogel before calendering.
4. The manufacturing method according to claim 1, It is characterized in that The solvent A is an ionic liquid, a mixed solvent formed by an ionic liquid and an organic solvent, an amine oxide system, a carbamate system, an alkaline solution, an alkali / urea aqueous solution, an alkali / thiourea aqueous solution, a liquid ammonia / NH 4 One or more of SCN and acid solution. Preferably, the ionic liquid is a molten salt formed by substituted or unsubstituted imidazolium or pyridinium cations and anions and having a melting point below 100°C. Preferably, the substituent on the imidazole or pyridinium cation is C 1-6 Alkyl, C 1-6 The anion is one or more of an alkyl acid ion, a halide ion, and an organic phosphate ion. For example, the ionic liquid is selected from one or more of 1-allyl-3-methylimidazolium chloride solution, 1-butyl-3-methylimidazolium acetate solution and 1-ethyl-3-methylimidazolium acetate solution. Preferably, the concentration of the ionic liquid is 50 wt% to 100 wt%.
5. The manufacturing method according to claim 4, It is characterized in that The organic solvent is selected from one or more of N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, acetone, tetrahydrofuran, pyridine, chloroform, dichloromethane and alcohols. Optionally, the alcohols are such as ethanol, methanol and isopropanol. Optionally, the mixed solvent formed by the ionic liquid and the organic solvent is, for example, N,N-dimethylacetamide / lithium chloride. Optionally, the amine oxide system is N-methylmorpholine oxide. Optionally, the alkaline solution is an aqueous sodium hydroxide solution and / or an aqueous potassium hydroxide solution. Optionally, the acid solution is selected from one or more of a phosphoric acid solution, a sulfuric acid solution, and an acetic acid solution.
6. The manufacturing method according to claim 1, It is characterized in that The solvent B in step 3 is selected from one or more of water, ethanol, ionic liquid / water, and ionic liquid / ethanol. Optionally, in the ionic liquid / water or ionic liquid / ethanol, the content of the ionic liquid is 5% to 80%.
7. The manufacturing method according to claim 1, It is characterized in that Before step 1, the method further includes placing the cellulose raw material in an oven for drying. Preferably, the temperature of the solvent A is 100-120° C., and the soaking time is 5 s to 90 s. For example, the filter paper is placed in a vacuum oven at 80° C. to dry for 48 hours, and then the filter paper is immersed in an ionic liquid 1-ethyl-3-methylimidazolium acetate (EmimAc) solution at 110° C. for 30 seconds.
8. The manufacturing method according to claim 1, It is characterized in that In step 2, the cellulose soaked with solvent A is sequentially laid on a mold frame for hot pressing. The hot pressing conditions are: pressing at a pressure of 8.0 to 8.5 MPa for 40 to 80 minutes in a vacuum laminating machine at 100 to 120°C. For example, three layers of filter paper soaked with ionic liquid were sequentially laid on a 1 mm thick mold frame, and then pressed at a pressure of 8.2 MPa for 60 min in a vacuum laminator at 110°C.
9. The manufacturing method according to claim 1, It is characterized in that The cellulose is selected from one or more of microcrystalline cellulose, pulp, paper, plant straw, grass plants, Chinese medicine residues, waste wood chips, bagasse, reeds, corn cobs, fruit shells, plant stems and leaves, wood powder, sawdust and bamboo. Optionally, the pulp is selected from one or more of cotton pulp, wood pulp, bamboo pulp and straw pulp. Optionally, the cellulose content of the paper is greater than 90%, for example, the paper is selected from one or more of qualitative filter paper, absorbent paper, toilet paper and A4 printing paper. Optionally, the plant straw is selected from one or more of wheat straw, corn straw, cotton straw, soybean straw, sorghum straw and rice straw. Optionally, the grass plant is selected from one or more of foxtail grass, pennisetum, and barnyard grass.
10. A high-strength, high-transparency and high-haze cellulose film, It is characterized in that The cellulose film is prepared by the method for producing a high-strength, high-transparency and high-haze cellulose film according to any one of claims 1 to 9. Preferably, the cellulose film has a light transmittance of >80%, a haze of >50%, a tensile strength of >250 MPa, and an elongation at break of >10%.