Schiff base-containing siloxane-coated inorganic flame retardant as well as preparation method and application thereof
Through the coating technology of Schiff base and siloxane, the problem of insufficient carbon-forming capacity of inorganic flame retardants is solved, and efficient flame retardant performance is achieved, which is suitable for fire-retardant applications of polymer materials.
Patent Information
- Application Number
- CN202410945881.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
AI Technical Summary
The existing inorganic flame retardants have insufficient carbon-forming capacity in polymer materials, resulting in limited flame retardant performance, and traditional coating technology has limited carbon-forming effect when improving environmental resistance.
Using Schiff base as the coating material, the coating structure is formed by combining with siloxane, and the thermally induced self-crosslinking properties of Schiff base enhances the carbon-forming ability of the polymer chain, and the hydrolysis and condensation reaction is used to form a network structure to enhance it. Flame retardant properties of inorganic substances.
It significantly improves the carbon-forming ability and flame-retardant properties of inorganic flame retardant, enhances the fire-retardant properties of polymer materials, and has simple preparation methods, wide application range, and large output. The product has excellent flame-retardant carbon-forming effects.
Smart Images

Figure CN118909311A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardant polymer materials, and in particular to a Schiff base-coated flame retardant, and in particular to a siloxane-coated inorganic flame retardant containing a Schiff base, a preparation method thereof, and application thereof in flame retardant polymers. Background Art
[0002] Polymer materials have been widely used in aerospace, electronics, construction, biomedicine and other fields due to their excellent mechanical strength, heat resistance and corrosion resistance. The wide range of applications of polymers requires them to have good flame retardant properties to meet the fire protection requirements of different application scenarios. At present, adding flame retardants has become a common flame retardant method for polymer materials due to its flexible design and wide application scenarios.
[0003] Traditionally, many phosphorus- and nitrogen-containing inorganic substances and hydroxides have good flame retardant effects and are often used as flame retardants. However, during use, the flame retardant effect of these inorganic substances is limited, and some more active substances will limit the use scenarios of flame retardants. Therefore, inorganic coating is the preferred technology to improve flame retardant properties and increase application areas. Inorganic coating technology uses inorganic substances as coating materials and coats inorganic flame retardants through methods such as chemical deposition. Although this method can reduce the hygroscopicity of the flame retardant itself and improve the environmental resistance of the flame retardant, its flame retardant efficiency is limited and will result in poor dispersion of flame retardants in the material. Compared with organic coating technology, since polymers (thermosetting resins such as phenolic resins, melamine resins, and urea-formaldehyde resins) are mostly used as coating materials, the generated flame retardants have better flame retardant effects and good dispersibility. However, most coating technologies focus on improving the environmental resistance of flame retardants, and the carbonization effect they bring is limited. Therefore, a coating technology is needed to improve the flame retardant efficiency of inorganic flame retardants and improve the carbon-forming ability of flame retardants. The Schiff base structure has the property of heat-induced self-crosslinking during the combustion process, which makes the polymer chain self-crosslinked, thereby enhancing the carbon-forming ability of the material, which provides a good development idea for flame retardant technology.
[0004] Therefore, how to provide a siloxane-coated inorganic flame retardant containing a Schiff base, that is, to invent a coating technology that can improve the carbon-forming ability of inorganic flame retardants and use it to improve the flame retardant properties of polymer materials is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0005] In view of this, the present invention provides a Schiff base-containing siloxane-coated inorganic flame retardant with simple preparation operation and excellent flame retardant effect, and a preparation method and application thereof.
[0006] It should be noted that coating flame retardants with flame retardant effects is currently a common means of improving the preparation of flame retardants, which can improve the flame retardant effect of flame retardants through the coating. Commonly, coating inorganic substances with gas-phase flame retardant effects with substances with carbon-forming effects can improve the flame retardant ability of flame retardants in the condensed phase. The imine (-CH=N-) bonds on Schiff base polymers can be rearranged and cyclized at high temperatures to generate nitrogen-containing six-membered heterocyclic compounds, resulting in self-crosslinking of polymer chains to form a stable network with excellent carbon-forming effects. In addition, the siloxane structure can undergo hydrolysis and condensation reactions in a specific environment, which is a good process for coating inorganic substances.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The first technical purpose of the present invention is to provide a siloxane-coated inorganic flame retardant containing a Schiff base, wherein the siloxane-coated inorganic flame retardant containing a Schiff base is obtained by hydrolyzing and coating an inorganic flame retardant with a siloxane intermediate containing a Schiff base; specifically, the siloxane-coated inorganic flame retardant containing a Schiff base has a structure as shown in Formula I:
[0009]
[0010] Wherein, R includes phosphorus-containing inorganic substances, nitrogen-containing inorganic substances, and metal hydroxides.
[0011] Preferably, R is selected from at least one of ammonium polyphosphate, red phosphorus, melamine cyanurate, melamine polyphosphate, aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite.
[0012] The second technical purpose of the present invention is to provide a method for preparing the above-mentioned siloxane-coated inorganic flame retardant containing Schiff base, comprising the following steps:
[0013] (1) γ-aminopropyltriethoxysilane (silane coupling agent KH550) and terephthalaldehyde are mixed and added into an organic solvent, and stirred to react under heating conditions;
[0014] (2) dispersing the inorganic substance uniformly in an organic solvent, and then adding the inorganic substance to the reaction system of step (1);
[0015] (3) adding water as a solvent and continuing the reaction;
[0016] (4) After the reaction is completed, pour out the reaction product, dry it, and cool it at room temperature to obtain a flame retardant;
[0017] (5) The flame retardant obtained in step (4) is washed, dried, cooled at room temperature, and crushed to obtain the Schiff base-containing siloxane-coated inorganic flame retardant.
[0018] The specific synthetic route is as follows:
[0019]
[0020] Optionally, in step (1), the molar ratio of terephthalaldehyde to KH550 is (1-1.2):(1.8-2.2); the organic solvent is selected from at least one of methanol, ethanol, acetone, toluene, xylene, tetrahydrofuran, N,N-dimethylformamide, and dimethyl sulfoxide; the reaction temperature is 85-95° C.; and the reaction time is 4-6.5 h.
[0021] Optionally, the ratio of the mass of the inorganic substance in step (2) to the total mass of terephthalaldehyde plus KH550 is (1.8-8.5):(0.9-2.2).
[0022] Optionally, the amount of water solvent added in step (3) is to adjust the solvent concentration to 75-90%; and the reaction time is 1-3h.
[0023] Optionally, in step (4), the drying temperature is 80-100° C. and the drying time is 20-30 h.
[0024] Optionally, in step (5), the washing solvent is ethanol, the washing time is 1-2 h / time, and the number of washing times is 2-4 times; the drying temperature is 60-85°C, and the drying time is 20-30 h.
[0025] The third technical purpose of the present invention is to provide the use of the above-mentioned siloxane-coated inorganic flame retardant containing Schiff base in the preparation of flame-retardant high molecular polymer products.
[0026] Specifically, the Schiff base-containing siloxane-coated inorganic flame retardant can be used to prepare flame-retardant high molecular polymer materials.
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0028] 1. The Schiff base bond exists in the siloxane-coated inorganic flame retardant containing a Schiff base disclosed in the present invention, which can form a network structure through thermal cross-linking, so that the combustible small molecules produced by thermal decomposition are converted into residual carbon, thereby improving the carbon-forming ability of the flame retardant.
[0029] 2. The siloxane-coated inorganic flame retardant containing a Schiff base disclosed in the present invention has a siloxane structure in its coating, which can be hydrolyzed and polymerized on the surface of the inorganic material to form a network coating structure to improve the flame retardant properties of the inorganic material.
[0030] 3. The preparation method of the Schiff base-containing siloxane-coated inorganic flame retardant disclosed in the present invention is simple, has a wide range of applications, and has a large output. The obtained product has an excellent flame retardant and carbonizing effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0032] Figure 1 It is the infrared spectra of terephthalaldehyde, KH550 and KP in Example 1 of the present invention.
[0033] Figure 2 It is the infrared spectra of ammonium polyphosphate, KP and KPAPP in Example 1 of the present invention.
[0034] Figure 3 It is the X-ray diffraction pattern of ammonium polyphosphate and KPAPP in Example 1 of the present invention.
[0035] Figure 4 This is a scanning electron microscope image of ammonium polyphosphate and KPAPP in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0038] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0039] The invention discloses a method for preparing a siloxane-coated inorganic flame retardant containing a Schiff base.
[0040] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that without certain specific details, the present application can be implemented equally. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail to highlight the purport of the present application. Under the premise of not conflicting, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the technical scheme obtained belongs to the content disclosed in the embodiments of the present application.
[0041] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0042] Example 1
[0043] A method for preparing a siloxane-coated ammonium polyphosphate flame retardant containing a Schiff base, specifically comprising the following steps:
[0044] (1) 110.5 g (0.5 mol) of KH550 and 33.5 g (0.25 mol) of terephthalaldehyde were mixed and added to 200 g of solvent, heated to 95° C., and reacted for 5 hours to obtain the intermediate KP;
[0045] (2) 243 g of ammonium polyphosphate was added to 300 g of solvent and dispersed evenly, and then added to the reaction in the first step;
[0046] (3) Add 150 g of water and continue the reaction for 1 h;
[0047] (4) After the reaction is completed, pour out the reaction product, dry it at 80°C for 24 hours, and cool it at room temperature;
[0048] (5) The flame retardant was washed twice with cold ethanol, dried at 80° C. for 20 h, cooled at room temperature, and crushed to obtain a siloxane-coated ammonium polyphosphate flame retardant (KPAPP) containing a Schiff base.
[0049] Example 2
[0050] A method for preparing a siloxane-coated red phosphorus flame retardant containing a Schiff base, specifically comprising the following steps:
[0051] (1) 11.05 g of KH550 and 3.35 g of terephthalaldehyde were mixed and added to 20 g of solvent, heated to 85° C., and reacted for 4.5 hours;
[0052] (2) 24.3 g of red phosphorus was added to 50 g of solvent and dispersed evenly, and then added to the reaction in the first step;
[0053] (3) Add 10 g of water and continue the reaction for 1 h;
[0054] (4) After the reaction is completed, pour out the reaction product, dry it at 100°C for 28 hours, and cool it at room temperature;
[0055] (5) The flame retardant was washed twice with cold ethanol, dried at 75° C. for 22 h, cooled at room temperature, and crushed to obtain a siloxane-coated red phosphorus flame retardant containing a Schiff base.
[0056] Example 3
[0057] A method for preparing a Schiff base-containing siloxane-coated aluminum hydroxide flame retardant specifically comprises the following steps:
[0058] (1) 22.1 g of KH550 and 6.7 g of terephthalaldehyde were mixed and added to 20 g of solvent, heated to 95° C., and reacted for 6 hours;
[0059] (2) 51.8 g of aluminum hydroxide was added to 50 g of solvent and dispersed evenly, and then added to the reaction in the first step;
[0060] (3) Add 20 g of water and continue the reaction for 2.5 h;
[0061] (4) After the reaction is completed, pour out the reaction product, dry it at 95°C for 30 hours, and cool it at room temperature;
[0062] (5) The flame retardant was washed once with cold ethanol, dried at 60° C. for 26 h, cooled at room temperature, and crushed to obtain a siloxane-coated aluminum hydroxide flame retardant containing a Schiff base.
[0063] Characterization of Example 1
[0064] The Fourier transform infrared spectra of terephthalaldehyde, KH550 and KP are shown in Figure 1 As shown. 815cm was observed in KP -1 The absorption peak at 1070 cm-1 corresponds to the benzene ring in terephthalaldehyde. -1 The absorption peak at 1690 cm corresponds to the Si-O bond in KH550. -1 The C=O bond at 1446 cm -1 The NH at the position disappears in KP, and a Schiff base bond is generated in KP (1653 cm -1 ) and CH bond (1566cm -1 ), which shows that the reaction of the coating is in line with the expected design.
[0065] Fourier transform infrared spectra of ammonium polyphosphate, KP, and KPAPP Figure 2In KPAPP, the C=N from KP is retained, and the POP, PO, and P=O bonds from APP are at 799 cm -1 、880cm -1 and 1248cm -1 The flame retardant monomer KPAPP containing Schiff base-coated ammonium polyphosphate was successfully synthesized.
[0066] like Figure 3 As shown, the crystal structures of ammonium polyphosphate and KPAPP were characterized using X-ray diffraction patterns. The peak in KPAPP is the same as the signal peak of ammonium polyphosphate, the peak intensity has not changed significantly, and no other new peaks have appeared, which shows that the coating has not changed the crystal structure of ammonium polyphosphate, thus indicating that KPAPP meets the expected design structure.
[0067] like Figure 4 As shown in the figure, the microstructure of ammonium polyphosphate and KPAPP was observed using a scanning electron microscope. It can be seen that the particles of inorganic ammonium polyphosphate present a typical crystal structure, and the surface of KPAPP particles is obviously wrapped with an object, which indicates that the coating is successfully coated on the surface of inorganic ammonium polyphosphate. In summary, a siloxane-coated inorganic flame retardant KPAPP containing a Schiff base was successfully synthesized.
[0068] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following experimental examples and comparative examples are provided to further illustrate the technical excellence of the present invention, but they should not be construed as limitations of the present invention. Other improvements made by those skilled in the art based on the above-mentioned invention without inventive work are also deemed to fall within the scope of protection of the present invention.
[0069] Experimental Example 1: Preparation of basic flame retardant composite materials
[0070] E51 bisphenol A epoxy resin was selected as the flame retardant matrix, and diaminodiphenylmethane (DDM) was selected as the curing agent of the epoxy resin. The mass ratio of epoxy resin to curing agent was epoxy resin: curing agent = 4:1. After the epoxy resin was stirred at 125°C until it had good fluidity, the siloxane-coated ammonium polyphosphate flame retardant (KPAPP) containing Schiff base prepared in Example 1 was added according to the total mass ratio of 3wt%, 5wt% and 7wt%; after the flame retardant was completely dissolved in the epoxy resin, the temperature was lowered to 75°C, and the curing agent was added and continued to be stirred until fully dispersed. Finally, the fully stirred mixture was vacuum treated to remove bubbles, poured into a polytetrafluoroethylene mold sprayed with a release agent, and a heat treatment procedure of 120°C / 2h, 150°C / 2h, and 180°C / 2h was performed to obtain a cured flame retardant epoxy resin composite material.
[0071] Comparative Example 1: Pure Epoxy Resin
[0072] Bisphenol A type E51 epoxy resin was used to prepare pure epoxy resin as a comparative example.
[0073] Comparative test of flame retardancy between Experimental Example 1 and Comparative Example 1:
[0074] In the present invention, the UL-94 vertical combustion test adopts the GB / T 2408-2008 standard; the limiting oxygen index test adopts the GB / T2406-93 standard. The basic flame retardant composite material prepared in Example 1 of the present invention and pure epoxy resin are tested and compared, and the results are shown in the following table.
[0075] Table 1 Performance test results
[0076]
[0077] In the table, NR stands for No Grade, which is a flammable material.
[0078] As can be seen from the table, the Schiff base-containing siloxane-coated ammonium polyphosphate flame retardant (KPAPP) prepared in Experimental Example 1 can greatly improve the flame retardant properties of epoxy resin. Ammonium polyphosphate can be used as an acid source and a phosphorus source in an intumescent flame retardant system, and the Schiff base-containing siloxane coating can be used as a carbon source to form a good intumescent flame retardant system and enhance the flame retardant effect of ammonium polyphosphate. A 5% addition of flame retardant can make the epoxy resin reach a V-1 grade in a vertical burning test. And because the Schiff base bonds present in the flame retardant have a self-crosslinking carbon-forming effect, the carbon-forming properties of the matrix are continuously improved during combustion to form a flame-retardant isolation zone. Moreover, the honeycomb cavity formed by high-temperature cross-linking encapsulates a large amount of combustible small molecules and heat, which effectively prevents heat transfer and smoke release. With the increase of flame retardant content, the epoxy resin reaches V-0 grade at 7% flame retardant addition, and the limiting oxygen index increases to 29.3%. The condensed phase flame retardant effect of Schiff base carbonization and the gas phase flame retardant effect of ammonium polyphosphate enable the flame retardant to play a high efficiency flame retardant role in epoxy resin composite materials.
[0079] In addition, the coating formed by hydrolysis polymerization improves the dispersion of flame retardant in epoxy resin. Adding 7% flame retardant can increase the impact strength of epoxy resin from 17.85KJ / m 2 Increased to 37.75KJ / m 2 The improvement of impact strength is mainly attributed to the network coating structure formed by the hydrolysis of Schiff base and siloxane in the molecule, which increases the cross-linking points and cross-linking density of the matrix and reduces the mobility of the main chain of the molecular matrix, making the matrix show good impact resistance.
[0080] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A siloxane-coated inorganic flame retardant containing a Schiff base, characterized in that: The Schiff base-containing siloxane-coated inorganic flame retardant is obtained by hydrolyzing and coating an inorganic flame retardant with a Schiff base-containing siloxane intermediate; specifically, the Schiff base-containing siloxane-coated inorganic flame retardant has a structure as shown in Formula I: Wherein, R includes phosphorus-containing inorganic substances, nitrogen-containing inorganic substances, and metal hydroxides.
2. The Schiff base-containing siloxane-coated inorganic flame retardant according to claim 1, characterized in that: R is selected from at least one of ammonium polyphosphate, red phosphorus, melamine cyanurate, melamine polyphosphate, aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite.
3. A method for preparing the Schiff base-containing siloxane-coated inorganic flame retardant according to claim 1, characterized in that: The method specifically comprises the following steps: (1) γ-aminopropyltriethoxysilane (silane coupling agent KH550) and terephthalaldehyde are mixed and added into an organic solvent, and heated and stirred for reaction; (2) dispersing the inorganic substance uniformly in an organic solvent, and then adding the inorganic substance to the reaction system of step (1); (3) adding water as a solvent and continuing the reaction; (4) After the reaction is completed, pour out the reaction product, dry it, and cool it at room temperature to obtain a flame retardant; (5) The flame retardant obtained in step (4) is washed, dried, cooled at room temperature, and crushed to obtain the Schiff base-containing siloxane-coated inorganic flame retardant.
4. The method for preparing the Schiff base-containing siloxane-coated inorganic flame retardant according to claim 3, characterized in that: In step (1), the molar ratio of terephthalaldehyde to KH550 is (1-1.2):(1.8-2.2); The organic solvent is selected from at least one of methanol, ethanol, acetone, toluene, xylene, tetrahydrofuran, N,N-dimethylformamide and dimethyl sulfoxide; The reaction temperature is 85-95°C; The reaction time is 4-6.5h.
5. The method for preparing the Schiff base-containing siloxane-coated inorganic flame retardant according to claim 3, characterized in that: In step (2), the ratio of the mass of the inorganic substance to the total mass of terephthalaldehyde plus KH550 is (1.8-8.5):(0.9-2.2).
6. The method for preparing the Schiff base-containing siloxane-coated inorganic flame retardant according to claim 3, characterized in that: In step (3), the amount of the aqueous solvent added is to adjust the solvent concentration to 75-90%; The reaction time is 1-3h.
7. The method for preparing the Schiff base-containing siloxane-coated inorganic flame retardant according to claim 3, characterized in that: In step (4), the drying temperature is 80-100° C. and the drying time is 20-30 hours.
8. The method for preparing the Schiff base-containing siloxane-coated inorganic flame retardant according to claim 3, characterized in that: In step (5), the washing solvent is ethanol, the washing time is 1-2h / time, and the number of washing times is 2-4 times; The drying temperature is 60-85℃ and the drying time is 20-30h.
9. Use of the Schiff base-containing siloxane-coated inorganic flame retardant as claimed in claim 1 in the preparation of flame-retardant high molecular polymer products.
Citation Information
Cited By
Solvent-resistant antirust anticorrosive biological resin coating and preparation method thereof
CN119708955A
Flame-retardant PC (polycarbonate) and ABS (acrylonitrile-butadiene-styrene) composite material for automotive trim
CN122502849A