Preparation method of phosphorus-containing flame-retardant N-phenylmaleimide and its application in heat-resistant flame-retardant ABS resin
The preparation of phosphorus-containing flame retardant N-phenylmaleimide by anionic polymerization solves the problems of poor thermal stability and fire safety hazards in high-temperature environments, and achieves the improvement of heat resistance and flame retardant performance of ABS resin , simplified process, environmentally friendly and pollution-free, suitable for industrial applications.
Patent Information
- Application Number
- CN202310720230.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-06-19
AI Technical Summary
The existing ABS resin has poor thermal stability and high fire safety risks in high temperature environments. The existing thermal flame retardant modifiers have complex processes, many pollutions and unstable effects, making it difficult to meet the application requirements of polymer materials in the European and American markets.
Anionic polymerization method is used to prepare phosphorus-containing flame retardant N-phenylmaleimide, and the macromolecular phosphorus-based flame retardant is synthesized through allylphosphate diester, styrene and 1,3-butadiene, and N -phenylmaleimide copolymerizes to form phosphorus-containing flame retardant N-phenylmaleimide, used to modify ABS resins, and form an interpenetrating polymer network structure to improve heat resistance and flame retardant properties.
It significantly improves the heat resistance and flame retardant properties of ABS resin, improves the durability and flame retardant effects of heat resistance, simplifies the process and discharges of environmentally friendly and harmless substances, and is suitable for industrial production.
Smart Images

Figure CN116769117B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heat-resistant and flame-retardant modification of polymers, and in particular to a method for preparing phosphorus-containing flame-retardant N-phenylmaleimide and a method for modifying the heat-resistant and flame-retardant property of ABS resin. Background Art
[0002] At present, ABS resin is widely used in many fields such as toys, decorations, consumer appliances and auto parts. However, as a common disadvantage of general polymer materials, ABS also has problems such as poor thermal stability and fire safety hazards during use. In an environment with high temperature requirements, its application is greatly limited. However, imide polymers have good heat resistance due to the presence of five-membered rings in their structure and are widely concerned. N-phenylmaleimide, as one of them, is a new monomer developed in recent years to improve the heat resistance of resin matrix. Secondly, phosphorus-based flame retardants will not generate a large amount of smoke, dioxins and corrosive gases when burning, which can meet the requirements of the "Directive on the Restriction of the Use of Certain Hazardous Substances in Electrical and Electronic Equipment" (abbreviated as ROHS) issued by the European Union in 2003, avoiding domestic toys and home appliances from being rejected by the European Union market, and greatly promoting the market share of products in overseas markets such as Europe and the United States. Therefore, designing and developing green and efficient heat-resistant flame retardant modifiers has become a problem to be solved in this field.
[0003] In the prior art, the research on heat-resistant flame-retardant modifiers of imide is mainly prepared by copolymerization. For example, ZL 200710069041.6 discloses a method of preparing St / AN / N-PMI ternary copolymers as heat-resistant modifiers for general polymer materials such as heat-resistant polymers and PVC by emulsion polymerization, mixing N-phenylmaleimide, styrene, acrylonitrile, chain transfer agent, suspending agent, and initiator, adding them into water, reacting at 20-120°C and pressure 0.05-0.3MPa for 0.5-10 hours. Hu Yimin et al. synthesized a styrene / N-phenylmaleimide / maleic anhydride terpolymer (St / N-PMI / MAH) with a St content of 35% to 50%, an N-PMI content of 48% to 63%, and a MAH content of 2% for use as a heat-resistant modifier for engineering plastics such as PA and PPO (Journal of Chemistry in Universities, 2009, 30(12): 2496-2501). CN101503545B discloses a composition of a heat-resistant flame-retardant maleimide resin containing halogen substituents and a preparation method thereof. The composition of the heat-resistant maleimide resin containing halogen substituents is 100 parts by mass, and contains 10 to 65 parts of the heat-resistant maleimide resin containing halogen substituents, 30 to 55 parts of graft polymerization of conjugated diene rubber grafted with aromatic vinyl monomers, nitrile vinyl monomers or copolymerizable acrylate monomers, and 5 to 35 parts of a binary copolymer of aromatic vinyl monomers and nitrile vinyl monomers. The composition, as a material with excellent heat-resistant and flame-retardant properties, can be widely used in heat-resistant and flame-retardant modification of materials such as ABS, PC, and PBT.
[0004] Although the above patents and documents have achieved significant results in improving the heat resistance and flame retardancy of resins such as ABS, PVC, PA and PPO, most of these modified copolymers adopt emulsion polymerization, which has many post-processing processes and is prone to dust formation, causing losses and pollution; secondly, there are certain differences in the surface properties of these copolymer modifiers and resins, resulting in poor stability and durability of heat resistance and flame retardant effects; finally, these copolymers can only be used as single modifiers for general plastics such as ABS and PVC, and there has been no report on high-molecular functionalized N-phenylmaleimide heat-resistant and flame-retardant modifiers that integrate heat resistance and flame retardancy. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a preparation method of phosphorus-containing flame-retardant N-phenylmaleimide and its application in heat-resistant flame-retardant ABS resin.
[0006] In order to solve the above technical problems, the present invention provides a phosphorus-containing flame-retardant N-phenylmaleimide, the general structural formula of which is shown in Formula I:
[0007]
[0008] In formula I, R is any alkyl group of C1 to C8; PS is a homopolymer of styrene; B is 1,3-butadiene; n and m are the number of repeating units, and n≥1, m≥1. n and m are both positive integers.
[0009] Specifically:
[0010]
[0011]
[0012] As an improvement of the phosphorus-containing flame-retardant N-phenylmaleimide of the present invention: the number average molecular weight of the phosphorus-containing flame-retardant N-phenylmaleimide is 20,000 to 50,000, and the ratio of the weight average molecular weight to the number average molecular weight is 3.43 to 4.12.
[0013] The present invention also provides a method for preparing the phosphorus-containing flame-retardant N-phenylmaleimide, comprising the following steps:
[0014] (1) Preparation of macromolecular phosphorus flame retardants:
[0015] Under the protection of inert gas, add the first raw material system to the solvent I, heat it to 60-70°C, then add the first polymerization initiator, keep the temperature at 60-70°C for 180-240min to obtain the first block system; then add the second raw material system to the first block system, heat it to 75-85°C for 80-100min, then add 1,3-butadiene for end-capping (fully react until no free monomer ---- 1,3-butadiene exists), wash and dry to obtain the macromolecular phosphorus flame retardant;
[0016] The first polymerization initiator is a hydrocarbyl monolithium compound;
[0017] The first raw material system is composed of allyl phosphate diester and structure regulator I, and the mass ratio of allyl phosphate diester to structure regulator I is 100: (0.7-0.9);
[0018] 5.7-11.4 mmol of the first polymerization initiator is used for every 1000 g of allyl phosphate diester;
[0019] The second raw material system consists of styrene and structure regulator II;
[0020] The mass ratio of the allyl phosphate diester to styrene and structure regulator II in the second raw material system is 100:(10-20):(0.2-0.4);
[0021] The mass ratio of the allyl phosphate diester to the 1,3-butadiene is 100:(1-3);
[0022] The structure regulator I and the structure regulator II are both polar organic compounds, and the structure regulator I and the structure regulator II are the same polar organic compound;
[0023] (2) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0024] Under the protection of inert gas, N-phenylmaleimide, a molecular weight regulator and the macromolecular phosphorus flame retardant obtained in step (1) are added to solvent II, and a second polymerization initiator is added when the system is heated to 70-80° C. to react for 120-180 minutes, and then a terminator is added to terminate the reaction, and the phosphorus-containing flame-retardant N-phenylmaleimide is obtained after suction filtration, washing, purification and drying;
[0025] The second polymerization initiator is an organic peroxide;
[0026] The mass ratio of the N-phenylmaleimide, the molecular weight regulator, the macromolecular phosphorus flame retardant, and the second polymerization initiator is 100:(0.1-0.3):(30-40):(0.05-0.1).
[0027] Note: The polymerization reaction in the above steps (1) and (2) is carried out in an oxygen-free, water-free environment and under the protection of an inert gas.
[0028] As an improvement to the preparation method of the phosphorus-containing flame-retardant N-phenylmaleimide of the present invention, in step (1):
[0029] The allyl phosphate diester is any one of dimethyl allyl phosphate (preferred), diethyl allyl phosphate, dipropyl allyl phosphate, dibutyl allyl phosphate, dipentyl allyl phosphate, dihexyl allyl phosphate, diheptyl allyl phosphate or dioctyl allyl phosphate;
[0030] The first polymerization initiator (hydrocarbyl monolithium compound) is any one of n-butyllithium (preferably), sec-butyllithium, methylbutyllithium, phenylbutyllithium, naphthalenelithium, cyclohexyllithium, and dodecyllithium;
[0031] The structure regulator I and the structure regulator II (polar organic compound) are any one of diethylene glycol dimethyl ether, tetrahydrofuran (preferably), ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether and triethylamine.
[0032] As a further improvement of the preparation method of the phosphorus-containing flame-retardant N-phenylmaleimide of the present invention, in step (2):
[0033] The second polymerization initiator (organic peroxide) is any one of dicumyl peroxide (preferably), cumyl hydroperoxide, benzoyl peroxide or di-tert-butyl peroxide;
[0034] The molecular weight regulator is any one of tert-decyl mercaptan, tert-dodecyl mercaptan (preferably), tert-tetradecyl mercaptan, and tert-hexadecyl mercaptan.
[0035] As a further improvement of the preparation method of the phosphorus-containing flame-retardant N-phenylmaleimide of the present invention, in step (2):
[0036] The terminator is any one of methanol, ethanol, propanol or butanol, and the mass ratio of the terminator to N-phenylmaleimide is (1-3):100.
[0037] Note: Taking methanol as an example, the hydroxyl groups in methanol have strong reducing properties and can easily combine with the active points of N-phenylmaleimide initiated by free radicals, making them inactive, thereby terminating the chain growth and stopping the polymerization reaction.
[0038] As a further improvement of the preparation method of the phosphorus-containing flame-retardant N-phenylmaleimide of the present invention, the solvent I in step (1) and the solvent II in step (2) are both hydrocarbon solvents selected from any one of pentane, hexane, octane, heptane, cyclohexane, benzene, toluene, xylene or ethylbenzene;
[0039] The mass ratio of solvent I to the allyl phosphate diester is (2-3):1;
[0040] The mass ratio of solvent II to the N-phenylmaleimide is (2-3): 1;
[0041] And solvent I and solvent II are selected from the same hydrocarbon solvent.
[0042] The present invention also provides a method for preparing an environmentally friendly heat-resistant and flame-retardant ABS resin, comprising the following steps:
[0043] Fully mixing ABS resin, phosphorus-containing flame-retardant N-phenylmaleimide, stabilizer and antioxidant in a mixer; the mass ratio of the ABS resin, phosphorus-containing flame-retardant N-phenylmaleimide, stabilizer and antioxidant is 100:(1-3):(0.1-0.3):(0.2-0.4);
[0044] The mixed materials are added into a screw kneader, and are subjected to reaction extrusion, cooling and granulation to obtain an environmentally friendly heat-resistant and flame-retardant ABS resin.
[0045] As an improvement of the preparation method of the environmentally friendly heat-resistant flame-retardant ABS resin of the present invention:
[0046] ABS resin is a terpolymer composed of styrene, acrylonitrile and 1,3-butadiene;
[0047] The stabilizer is a stearate (e.g. zinc stearate, magnesium stearate or calcium stearate);
[0048] The antioxidant is any one of 2,2'-methylenebis(4-methyl-6-tert-butylphenol), p(4-hydroxy.3,5-di-tert-butylphenyl) propionate, and tetrakis-[p.(3,5.di-tert-butyl.4.hydroxyphenyl) propionate].
[0049] As a further improvement of the preparation method of the environmentally friendly heat-resistant flame-retardant ABS resin of the present invention:
[0050] The temperature of the reaction extrusion is 180-210° C., and the screw speed is 30-50 rpm; the screw kneading machine is a single-screw extruder or a multi-screw extruder (preferably a twin-screw extruder).
[0051] The melt---the flow rate of the modified ABS resin (765) is 1.0-30.0 g / 10 min.
[0052] One of the purposes of the present invention is to provide a method for preparing phosphorus-containing flame-retardant N-phenylmaleimide. The invention firstly uses anionic polymerization to synthesize a reactive macromolecular "phosphorus" flame retardant from a small molecule flame retardant allyl phosphate diester, styrene and 1,3-butadiene; secondly, phosphorus-containing flame-retardant N-phenylmaleimide is prepared by copolymerizing N-phenylmaleimide and a reactive macromolecular "phosphorus" flame retardant.
[0053] The present invention also provides a phosphorus-containing flame-retardant N-phenylmaleimide as a polymer heat-resistant flame retardant, which can significantly improve the heat resistance and flame retardancy of ABS resin, thereby broadening the application range of ABS resin.
[0054] The "%" mentioned in the present invention refers to mass percentage.
[0055] As one aspect of the present invention, it relates to a phosphorus-containing flame-retardant N-phenylmaleimide, which is a linear block copolymer composed of N-phenylmaleimide, styrene, 1,3-butadiene and allyl phosphate diester, and its general structural formula is shown in the above formula I.
[0056] In the present invention, the first polymerization initiator is a hydrocarbon monolithium compound, namely RLi, wherein R is a saturated aliphatic hydrocarbon group, alicyclic hydrocarbon group, aromatic hydrocarbon group or a composite group of the above groups containing 1 to 20 carbon atoms. The hydrocarbon monolithium compound is selected from one of n-butyl lithium, sec-butyl lithium, methyl butyl lithium, phenyl butyl lithium, naphthalene lithium, cyclohexyl lithium and dodecyl lithium, preferably n-butyl lithium. The amount of organic lithium added is determined by the molecular weight of the designed polymer.
[0057] The second polymerization initiator described in the present invention is an organic peroxide selected from one of dicumyl peroxide (DCP), cumyl hydroperoxide, benzoyl peroxide (BPO) or di-tert-butyl peroxide, preferably dicumyl peroxide (DCP).
[0058] The structure regulator of the present invention is a polar organic compound that produces a solvation effect in the polymerization system, and can adjust the reactivity ratio of styrene and isoprene to make the two copolymerize randomly. This type of polar organic compound is selected from one of diethylene glycol dimethyl ether (DGE), tetrahydrofuran (THF), ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether (DME), and triethylamine, preferably tetrahydrofuran (THF).
[0059] The polymerization reaction of the present invention is carried out in an oxygen-free and water-free environment, preferably in an inert gas environment. The polymerization process is completed in a hydrocarbon solvent. The solvent of the present invention is a hydrocarbon solvent, which includes straight-chain alkanes, aromatic hydrocarbons and cycloalkanes. The hydrocarbon solvent is selected from pentane, hexane, octane, heptane, cyclohexane, benzene, toluene, xylene or ethylbenzene, preferably cyclohexane.
[0060] In the preparation process of the environmentally friendly heat-resistant flame-retardant ABS resin of the present invention, the ABS resin is a terpolymer composed of styrene, acrylonitrile and 1,3-butadiene, which can be a powdery or granular resin with a melt flow rate (MFR) of 1.0 to 30.0 g / 10 min; the screw kneader can be a single-screw extruder or a multi-screw extruder, preferably a twin-screw extruder; the stabilizer and antioxidant and other additives are only used to meet the requirements of stable processing of ABS resin, and these additives are not particularly limited, and conventional additives commonly used in the art can be used, such as the stabilizer is a stearate, such as zinc stearate, magnesium stearate or calcium stearate, preferably zinc stearate. The antioxidant is one of phenolic, hindered amine, and phosphorous acid diester antioxidants.
[0061] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0062] (1) The phosphorus-containing flame-retardant N-phenylmaleimide prepared by the present invention combines phenyl, imide groups and phosphorus-containing ester groups on a macromolecular chain by anionic polymerization and free radical solution polymerization, and the arrangement is regular, which will produce the superposition effect of "group effect" and "structural effect", and can greatly improve the efficiency of heat resistance and flame retardant modification of ABS resin.
[0063] (2) The phosphorus-containing flame-retardant N-phenylmaleimide prepared by the present invention has a certain affinity with the surface of ABS resin and can form an interpenetrating polymer network structure with ABS resin, thereby avoiding the migration and precipitation problems of small molecule heat-resistant agent N-phenylmaleimide or small molecule flame retardant allyl phosphate diester in the ABS resin matrix, thereby greatly improving the durability of heat-resistant effect and flame-retardant effect.
[0064] (3) The phosphorus-containing flame-retardant N-phenylmaleimide prepared by the present invention has the characteristics of no volatility, high carbon forming property and low amount of modified additives.
[0065] (4) The preparation method of the phosphorus-containing flame-retardant N-phenylmaleimide of the present invention is green and environmentally friendly, has no harmful substance emissions, has a short post-processing process, and is suitable for industrial production. DETAILED DESCRIPTION
[0066] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:
[0067] ⑴Source of raw materials:
[0068] ABS resin (765), mass ratio of styrene: acrylonitrile: 1,3-butadiene 65:13:22; PetroChina Daqing Petrochemical Company
[0069]
[0070] Other reagents are commercially available products.
[0071] ⑵The structural design of the Ф60 screw kneader is: divided into 9 sections, each section is 33 cm long, and the material is fed in the first section. ⑶Analysis and testing methods:
[0072] Determination of molecular weight and molecular weight dispersion index: 2414 gel permeation chromatograph (GPC) produced by Waters Company of the United States was used for determination. Polystyrene standard was used as calibration curve, mobile phase was tetrahydrofuran, column temperature was 40°C, sample concentration was 1 mg / ml, injection volume was 50 μL, elution time was 40 min, flow rate was 1 ml·min -1 .
[0073] Vicat softening temperature: measured according to the method described in GB / T 1633-2000.
[0074] Determination of oxygen index: Determine according to the method described in GB10707-1989.
[0075] Determination by vertical combustion method: Determine according to the method described in GB / T13488-1992.
[0076] Determination of elemental carbon and hydrogen: Determine according to the method described in GB / T 6040-2019.
[0077] Determination of mass-to-charge ratio: Determine according to the method described in GB / T 6040-2020.
[0078] Example 1
[0079] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0080] a. Preparation of macromolecular "phosphorus" flame retardant: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced three times, and 2000g of cyclohexane, 1000g of allyl dimethyl phosphate, and 7.0g of THF (tetrahydrofuran) were added to the polymerization reactor in sequence, stirred and mixed, and heated. When the temperature of the reactor reached 60°C, 5.7mmol of n-butyl lithium was added and reacted for 180min to obtain the first block system;
[0081] Then, 100 g of styrene and 2.0 g of THF were added to the first block system in the polymerization kettle, the temperature was raised to 75° C., and the reaction was carried out for 80 minutes. Finally, 10 g of 1,3-butadiene was added to the polymerization kettle for end-capping, and the reaction was carried out for 30 minutes until no free monomer (1,3-butadiene) was present. After washing (using cyclohexane for washing until 1,3-butadiene <2000 ppm was completed) and drying (drying at 60-70° C. to constant weight), a reactive macromolecular "phosphorus" flame retardant was obtained.
[0082] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced three times, and 2000g of cyclohexane, 1000g of N-phenylmaleimide, 300g of macromolecular "phosphorus" flame retardant, and 1.0g of tert-dodecyl mercaptan were added to the polymerization kettle in sequence, stirred, mixed, and heated. When the temperature of the polymerization kettle reached 70°C, 0.5g of DCP was added and reacted for 2.0h, and then 10g of methanol was added to terminate the reaction. The reaction was filtered, washed (washed with cyclohexane until the macromolecular "phosphorus" flame retardant was <5000ppm), purified and dried (adding sufficient activated carbon and drying at 80-90°C to constant weight), to obtain phosphorus-containing flame-retardant N-phenylmaleimide.
[0083] The structural formula is:
[0084]
[0085] Elemental analysis of phosphorus-containing flame-retardant N-phenylmaleimide C41H52O3N2P Theoretical value: C, 75.58; H, 7.99. Measured value: C, 75.27; H, 7.68.
[0086] Mass spectrum (ESI): m / z 654.12 (M+).
[0087] The phosphorus-containing flame-retardant N-phenylmaleimide obtained in this embodiment has an Mn of 20200 and an Mw / Mn of 3.43; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0088] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: 20000g of ABS (765) resin, 200g of phosphorus-containing flame-retardant N-phenyl maleimide, 20g of calcium stearate and 40g of antioxidant 1076 were added to a high-speed mixer and mixed at high speed for 15 minutes. The mixed materials were then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw were: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed was 30rpm, extrusion, cooling, and granulation were performed to obtain environmentally friendly heat-resistant flame-retardant ABS resin. Sampling analysis: Standard samples were prepared, and the test properties are shown in Table 1.
[0089] Example 2
[0090] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0091] a. Preparation of macromolecular "phosphorus" flame retardant: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced three times, and 2300g of cyclohexane, 1000g of allyl dimethyl phosphate, and 7.5g of THF were added to the polymerization kettle in sequence, stirred, mixed, and heated. When the temperature of the reactor reached 62°C, 7.1mmol of n-butyl lithium was added to react for 200min; then 130g of styrene and 2.6g of THF were added to the polymerization kettle, the temperature was raised to 77°C, and the reaction was carried out for 84min. Finally, 16g of 1,3-butadiene was added to the polymerization kettle for end-capping, and the reaction was carried out for 35min until no free monomer was present. After washing and drying, a macromolecular "phosphorus" flame retardant with reactive activity was obtained.
[0092] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced three times, and 2200g of cyclohexane, 1000g of N-phenylmaleimide, 320g of macromolecular "phosphorus" flame retardant, and 1.5g of tert-dodecyl mercaptan were added to the polymerization kettle in sequence, and the mixture was stirred and heated. When the temperature of the polymerization kettle reached 72°C, 0.6g of DCP was added and the reaction was carried out for 2.2h, and then 15g of methanol was added to terminate the reaction. After filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide was obtained.
[0093] The structural formula is:
[0094]
[0095] Elemental analysis of phosphorus-containing flame-retardant N-phenylmaleimide C41H52O3N2P Theoretical value: C, 75.58; H, 7.99. Measured value: C, 75.38; H, 7.72.
[0096] Mass spectrum (ESI): m / z 671.32 (M+).
[0097] The phosphorus-containing flame-retardant N-phenylmaleimide obtained in this embodiment has an Mn of 28,000 and an Mw / Mn of 3.61; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0098] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: 20000g of ABS (765) resin, 300g of phosphorus-containing flame-retardant N-phenyl maleimide, 30g of calcium stearate and 50g of antioxidant 1076 were added to a high-speed mixer and mixed at high speed for 16 minutes. The mixed materials were then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw were: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed was 35rpm, extrusion, cooling, and granulation were performed to obtain environmentally friendly heat-resistant flame-retardant ABS resin. Sampling analysis: Standard samples were prepared, and the test properties are shown in Table 1.
[0099] Example 3
[0100] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0101] a. Preparation of macromolecular "phosphorus" flame retardant: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 4 times, and 2500g of cyclohexane, 1000g of diethyl allyl phosphate, and 8.0g of THF were added to the polymerization kettle in sequence, stirred, mixed, and heated. When the temperature of the reactor reached 65°C, 9.3mmol of n-butyl lithium was added to react for 210min; then 160g of styrene and 3.0g of THF were added to the polymerization kettle, the temperature was raised to 80°C, and the reaction was carried out for 90min. Finally, 21g of 1,3-butadiene was added to the polymerization kettle for end-capping, and the reaction was carried out for 40min until no free monomer was present. After washing and drying, a macromolecular "phosphorus" flame retardant with reactive activity was obtained.
[0102] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 4 times, and 2500g of cyclohexane, 1000g of N-phenylmaleimide, 350g of macromolecular "phosphorus" flame retardant, and 2.0g of tert-dodecyl mercaptan were added to the polymerization kettle in sequence, and the mixture was stirred and heated. When the temperature of the polymerization kettle reached 75°C, 0.8g of DCP was added and the reaction was carried out for 2.5h, and then 20g of methanol was added to terminate the reaction. After filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide was obtained.
[0103] The structural formula is:
[0104]
[0105] Elemental analysis of phosphorus-containing flame-retardant N-phenylmaleimide C43H56O3N2P Theoretical value: C, 75.99; H, 8.25. Measured value: C, 75.72; H, 8.17.
[0106] Mass spectrum (ESI): m / z 679.12 (M+).
[0107] The phosphorus-containing flame-retardant N-phenylmaleimide obtained in this embodiment has an Mn of 39,000 and an Mw / Mn of 3.85; in the general formula described in Formula I, R is ethyl (C2H5), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0108] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: 20000g of ABS (765) resin, 400g of phosphorus-containing flame-retardant N-phenyl maleimide, 40g of calcium stearate and 60g of antioxidant 1076 were added to a high-speed mixer and mixed at high speed for 17 minutes. The mixed materials were then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw were: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed was 40rpm, extrusion, cooling, and granulation were performed to obtain environmentally friendly heat-resistant flame-retardant ABS resin. Sampling analysis: Standard samples were prepared, and the test properties are shown in Table 1.
[0109] Example 4
[0110] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0111] a. Preparation of macromolecular "phosphorus" flame retardant: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 4 times, and 2800g of cyclohexane, 1000g of allyl dimethyl phosphate, and 8.5g of THF were added to the polymerization kettle in sequence, stirred, mixed, and heated. When the temperature of the reactor reached 67°C, 10.5mmol of n-butyl lithium was added to react for 230min; then 180g of styrene and 3.5g of THF were added to the polymerization kettle, the temperature was raised to 83°C, and the reaction was carried out for 95min. Finally, 26g of 1,3-butadiene was added to the polymerization kettle for end-capping, and the reaction was carried out for 45min until no free monomer was present. After washing and drying, a macromolecular "phosphorus" flame retardant with reactive activity was obtained.
[0112] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 4 times, and 2700g of cyclohexane, 1000g of N-phenylmaleimide, 380g of macromolecular "phosphorus" flame retardant, and 2.5g of tert-dodecyl mercaptan were added to the polymerization kettle in sequence, and the mixture was stirred and heated. When the temperature of the polymerization kettle reached 78°C, 0.9g of DCP was added and the reaction was carried out for 2.7h, and then 25g of ethanol was added to terminate the reaction. After filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide was obtained.
[0113] The structural formula is:
[0114]
[0115] Elemental analysis of phosphorus-containing flame-retardant N-phenylmaleimide C41H52O3N2P Theoretical value: C, 75.58; H, 7.99. Measured value: C, 75.36; H, 7.75.
[0116] Mass spectrum (ESI): m / z 684.12 (M+).
[0117] The phosphorus-containing flame-retardant N-phenylmaleimide obtained in this embodiment has an Mn of 46,000 and an Mw / Mn of 4.01; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0118] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: 20000g of ABS (765) resin, 500g of phosphorus-containing flame-retardant N-phenyl maleimide, 50g of calcium stearate and 70g of antioxidant 1076 were added to a high-speed mixer and mixed at high speed for 18 minutes. The mixed materials were then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw were: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed was 45rpm, extrusion, cooling, and granulation were performed to obtain environmentally friendly heat-resistant flame-retardant ABS resin. Sampling analysis: Standard samples were prepared, and the test properties are shown in Table 1.
[0119] Example 5
[0120] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0121] a. Preparation of macromolecular "phosphorus" flame retardant: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 5 times, and 3000g of cyclohexane, 1000g of dioctyl allyl phosphate, and 9.0g of THF were added to the polymerization kettle in sequence, stirred and mixed, and heated. When the temperature of the reactor reached 70°C, 11.4mmol of n-butyl lithium was added to the polymerization kettle and reacted for 240min; then 200g of styrene and 4.0g of THF were added to the polymerization kettle, the temperature was raised to 85°C, and the reaction was carried out for 100min. Finally, 30g of 1,3-butadiene was added to the polymerization kettle for end-capping, and the reaction was carried out for 50min until no free monomer was present. After washing and drying, a macromolecular "phosphorus" flame retardant with reactive activity was obtained.
[0122] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 5 times, and 3000g of cyclohexane, 1000g of N-phenylmaleimide, 400g of macromolecular "phosphorus" flame retardant, and 3.0g of tert-dodecyl mercaptan were added to the polymerization kettle in sequence, and the mixture was stirred and heated. When the temperature of the polymerization kettle reached 80°C, 1.0g of DCP was added and reacted for 3.0hr, and then 30g of ethanol was added to terminate the reaction. After filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide was obtained.
[0123] The structural formula is:
[0124]
[0125] Elemental analysis of phosphorus-containing flame-retardant N-phenylmaleimide: C41H52O3N2P: theoretical value: C, 83.31; H, 10.48. Measured value: C, 83.17; H, 10.15.
[0126] Mass spectrum (ESI): m / z 764.18 (M+).
[0127] The phosphorus-containing flame-retardant N-phenylmaleimide obtained in this embodiment has an Mn of 50,000 and an Mw / Mn of 4.12; in the general formula described in Formula I, R is an octyl group (C8H 17 ), B is 1,3-butadiene, n, m are the number of repeating units: n≥1, m≥1.
[0128] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: 20000g of ABS (765) resin, 600g of phosphorus-containing flame-retardant N-phenyl maleimide, 60g of calcium stearate and 80g of antioxidant 1076 were added to a high-speed mixer and mixed at high speed for 20 minutes. The mixed materials were then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw were: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed was 50rpm, extrusion, cooling, and granulation were performed to obtain environmentally friendly heat-resistant flame-retardant ABS resin. Sampling analysis: Standard samples were prepared, and the test properties are shown in Table 1.
[0129] Example 6
[0130] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0131] a. Preparation of macromolecular "phosphorus" flame retardant: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 5 times, and 3000g of cyclohexane, 1000g of allyl dimethyl phosphate, and 9.0g of THF were added to the polymerization kettle in sequence, stirred and mixed, and heated. When the temperature of the reactor reached 70°C, 11.4mmol of n-butyl lithium was added to the polymerization kettle and reacted for 240min; then 200g of styrene and 4.0g of THF were added to the polymerization kettle, the temperature was raised to 85°C, and the reaction was carried out for 100min. Finally, 30g of 1,3-butadiene was added to the polymerization kettle for end-capping, and the reaction was carried out for 50min until no free monomer was present. After washing and drying, a macromolecular "phosphorus" flame retardant with reactive activity was obtained.
[0132] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: First, in an 8L stainless steel reactor with a jacket, nitrogen was replaced 5 times, and 3000g of cyclohexane, 1000g of N-phenylmaleimide, 400g of macromolecular "phosphorus" flame retardant, and 3.0g of tert-dodecyl mercaptan were added to the polymerization kettle in sequence, and the mixture was stirred and heated. When the temperature of the polymerization kettle reached 80°C, 1.0g of DCP was added and the reaction was carried out for 3.0h, and then 30g of ethanol was added to terminate the reaction. After filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide was obtained.
[0133] The structural formula is:
[0134]
[0135] Elemental analysis of phosphorus-containing flame-retardant N-phenylmaleimide C41H52O3N2P Theoretical value: C, 75.58; H, 7.99. Measured value: C, 75.49; H, 7.83.
[0136] Mass spectrum (ESI): m / z 696.17 (M+).
[0137] The phosphorus-containing flame-retardant N-phenylmaleimide obtained in this embodiment has an Mn of 49,000 and an Mw / Mn of 4.09; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0138] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: 20000g of ABS (765) resin, 600g of phosphorus-containing flame-retardant N-phenyl maleimide, 60g of calcium stearate and 80g of antioxidant 1076 were added to a high-speed mixer and mixed at high speed for 20 minutes. The mixed materials were then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw were: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed was 50rpm, extrusion, cooling, and granulation were performed to obtain environmentally friendly heat-resistant flame-retardant ABS resin. Sampling analysis: Standard samples were prepared, and the test properties are shown in Table 1.
[0139] Comparative Example 1
[0140] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0141] a. Preparation of macromolecular "phosphorus" flame retardant: other conditions are similar to those in Example 1, except that allyl dimethyl phosphate is not added in the preparation process of the macromolecular "phosphorus" flame retardant, and only allyl methyl phosphate is added in an amount of 1000 g, that is: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 3 times, 2000 g of cyclohexane, 1000 g of allyl methyl phosphate, and 7.0 g of THF are added to the polymerization kettle in sequence, stirred and mixed, heated, and when the temperature of the reactor reaches 60°C, 5.7 mmol of n-butyl lithium is added to react for 180 min; then 100 g of styrene and 2.0 g of THF are added to the polymerization kettle, the temperature is raised to 75°C, and the reaction is carried out for 80 min, and finally 10 g of 1,3-butadiene is added to the polymerization kettle for end-capping, and the reaction is carried out for 30 min until no free monomer is present, and then washed and dried to obtain a macromolecular "phosphorus" flame retardant-1 with reactive activity.
[0142] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: Other conditions are similar to those in Example 1, except that in the preparation process of phosphorus-containing flame-retardant N-phenylmaleimide, instead of adding macromolecular "phosphorus" flame retardant, macromolecular "phosphorus" flame retardant-1 is added in an amount of 300 g, namely: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 3 times, 2000 g of cyclohexane, 1000 g of N-phenylmaleimide, 300 g of macromolecular "phosphorus" flame retardant, and 1.0 g of tert-dodecyl mercaptan are added to the polymerization reactor in sequence, stirred and mixed, heated, and when the polymerization reactor temperature reaches 70°C, 0.5 g of DCP is added and reacted for 2.0 hr, and then 10 g of methanol is added to terminate the reaction. After suction filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide-1 is obtained.
[0143] The phosphorus-containing flame-retardant N-phenylmaleimide-1 obtained in this comparative example has an Mn of 18000 and an Mw / Mn of 3.37; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0144] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: Other conditions are the same as those in Example 1, except that phosphorus-containing flame-retardant N-phenylmaleimide is not added during the preparation of the environmentally friendly heat-resistant flame-retardant ABS resin, but phosphorus-containing flame-retardant N-phenylmaleimide-1 is added in an amount of 200 g, that is, 20,000 g of ABS (765) resin, 200 g of phosphorus-containing flame-retardant N-phenylmaleimide-1, 20 g of calcium stearate and 40 g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 15 min. The mixed materials are then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw are 180, 180, 190, 190, 200, 210, 195, 185, and 180, respectively. The screw speed is 30 rpm, and the mixture is extruded, cooled, and granulated to obtain an environmentally friendly heat-resistant flame-retardant ABS resin. Sampling and analysis: Standard specimens were made and the test performance is shown in Table 1.
[0145] Comparative Example 2
[0146] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0147] a. Preparation of macromolecular "phosphorus" flame retardant: other conditions are similar to those in Example 2, except that 1,3-butadiene is not added during the preparation of the macromolecular "phosphorus" flame retardant, namely: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced three times, 2300g of cyclohexane, 1000g of allyl dimethyl phosphate, and 7.5g of THF are added to the polymerization kettle in sequence, stirred and mixed, and heated. When the temperature of the reactor reaches 62°C, 7.1mmol of n-butyl lithium is added to react for 200min; then 130g of styrene and 2.6g of THF are added to the polymerization kettle, the temperature is raised to 77°C, and the reaction is carried out for 84min, and then washed and dried to obtain macromolecular "phosphorus" flame retardant-2.
[0148] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: Other conditions are similar to those in Example 2, except that in the preparation process of phosphorus-containing flame-retardant N-phenylmaleimide, instead of adding macromolecular "phosphorus" flame retardant, macromolecular "phosphorus" flame retardant-2 is added in an amount of 320 g, namely: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 3 times, 2200 g of cyclohexane, 1000 g of N-phenylmaleimide, 320 g of macromolecular "phosphorus" flame retardant, and 1.5 g of tert-dodecyl mercaptan are added to the polymerization reactor in sequence, stirred and mixed, heated, and when the polymerization reactor temperature reaches 72° C., 0.6 g of DCP is added and reacted for 2.2 hr, and then 15 g of methanol is added to terminate the reaction. After suction filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide-2 is obtained. The phosphorus-containing flame-retardant N-phenylmaleimide-2 obtained in this comparative example has an Mn of 11000 and an Mw / Mn of 3.05; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0149] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: Other conditions are similar to those in Example 2, except that phosphorus-containing flame-retardant N-phenylmaleimide is not added during the preparation of the environmentally friendly heat-resistant flame-retardant ABS resin, but phosphorus-containing flame-retardant N-phenylmaleimide-2 is added in an amount of 300 g, that is, 20,000 g of ABS (765) resin, 300 g of phosphorus-containing flame-retardant N-phenylmaleimide-2, 30 g of calcium stearate and 50 g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 16 min. The mixed materials are then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw are 180, 180, 190, 190, 200, 210, 195, 185, and 180, respectively. The screw speed is 35 rpm, and the mixture is extruded, cooled, and granulated to obtain an environmentally friendly heat-resistant flame-retardant ABS resin. Sampling and analysis: Standard specimens were made and the test performance is shown in Table 1.
[0150] Comparative Example 3
[0151] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0152] a. Preparation of macromolecular "phosphorus" flame retardant: Other conditions are similar to those in Example 3, except that anionic polymerization is not used in the preparation process of the macromolecular "phosphorus" flame retardant, but free radical polymerization is used, that is, n-butyl lithium is not added, but DCP is added, that is: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 4 times, 2500g of cyclohexane, 1000g of diethyl allyl phosphate, and 8.0g of THF are added to the polymerization kettle in sequence, stirred and mixed, heated, and when the temperature of the reactor reaches 65°C, 9.3mmol DCP is added to react for 210min; then 160g of styrene and 3.0g of THF are added to the polymerization kettle, the temperature is raised to 80°C, and the reaction is carried out for 90min, and finally 21g of 1,3-butadiene is added to the polymerization kettle for end-capping, and the reaction is carried out for 40min until there is no free monomer, and then washed and dried to obtain a macromolecular "phosphorus" flame retardant-3 with reactive activity.
[0153] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: Other conditions are similar to those in Example 3, except that in the preparation process of phosphorus-containing flame-retardant N-phenylmaleimide, instead of adding macromolecular "phosphorus" flame retardant, macromolecular "phosphorus" flame retardant-3 is added in an amount of 350 g, that is: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 4 times, 2500 g of cyclohexane, 1000 g of N-phenylmaleimide, 3350 g of macromolecular "phosphorus" flame retardant, and 2.0 g of tert-dodecyl mercaptan are added to the polymerization reactor in sequence, stirred and mixed, heated, and when the temperature of the polymerization reactor reached 75°C, 0.8 g of DCP was added and reacted for 2.5 h, and then 20 g of methanol was added to terminate the reaction. After suction filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide-3 was obtained.
[0154] The phosphorus-containing flame-retardant N-phenylmaleimide-3 obtained in this comparative example has an Mn of 19500 and an Mw / Mn of 4.79; in the general formula described in Formula I, R is ethyl (C2H5), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0155] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: Other conditions are similar to those in Example 3, except that in the preparation process of the environmentally friendly heat-resistant flame-retardant ABS resin, phosphorus-containing flame-retardant N-phenylmaleimide is not added, but phosphorus-containing flame-retardant N-phenylmaleimide-3 is added in an amount of 400 g. That is, 20,000 g of ABS (765) resin, 400 g of phosphorus-containing flame-retardant N-phenylmaleimide-3, 40 g of calcium stearate and 60 g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 17 min. The mixed materials are then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw are: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed is 40 rpm, extrusion, cooling, and granulation are performed to obtain the environmentally friendly heat-resistant flame-retardant ABS resin. Sampling and analysis: Standard specimens were made and the test performance is shown in Table 1.
[0156] Comparative Example 4
[0157] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0158] a. Preparation of macromolecular "phosphorus" flame retardant: other conditions are similar to those in Example 4, except that styrene is not added during the preparation of the macromolecular "phosphorus" flame retardant, namely: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 4 times, 2800g of cyclohexane, 1000g of allyl dimethyl phosphate, and 8.5g of THF are added to the polymerization kettle in sequence, stirred and mixed, and heated. When the temperature of the reactor reaches 67°C, 10.5mmol of n-butyl lithium is added to react for 230min; then 26g of 1,3-butadiene is added to the polymerization kettle for end-capping, and the reaction is carried out for 45min until no free monomer is present. After washing and drying, a reactive macromolecular "phosphorus" flame retardant-4 is obtained.
[0159] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: Other conditions are similar to those in Example 4, except that in the preparation process of phosphorus-containing flame-retardant N-phenylmaleimide, instead of adding macromolecular "phosphorus" flame retardant, macromolecular "phosphorus" flame retardant-4 is added in an amount of 380 g, namely: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 4 times, 2700 g of cyclohexane, 1000 g of N-phenylmaleimide, 380 g of macromolecular "phosphorus" flame retardant, and 2.5 g of tert-dodecyl mercaptan are added to the polymerization reactor in sequence, stirred and mixed, heated, and when the polymerization reactor temperature reached 78°C, 0.9 g of DCP was added and reacted for 2.7 hours, and then 25 g of ethanol was added to terminate the reaction. After suction filtration, washing, purification and drying, phosphorus-containing flame-retardant N-phenylmaleimide-4 was obtained.
[0160] The phosphorus-containing flame-retardant N-phenylmaleimide-4 obtained in this comparative example has an Mn of 32,000 and an Mw / Mn of 3.86; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0161] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: Other conditions are similar to those in Example 4, except that in the preparation process of the environmentally friendly heat-resistant flame-retardant ABS resin, phosphorus-containing flame-retardant N-phenylmaleimide is not added, but phosphorus-containing flame-retardant N-phenylmaleimide-4 is added in an amount of 500 g. That is, 20,000 g of ABS (765) resin, 500 g of phosphorus-containing flame-retardant N-phenylmaleimide-4, 50 g of calcium stearate and 70 g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 18 min. The mixed materials are then directly added to a Φ60 screw kneader. The reaction temperatures (°C) of each section of the screw are: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed is 45 rpm, and the mixture is extruded, cooled, and granulated to obtain an environmentally friendly heat-resistant flame-retardant ABS resin. Sampling and analysis: Standard specimens were made and the test performance is shown in Table 1.
[0162] Comparative Example 5
[0163] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: The difference from the present invention is that in the preparation process of phosphorus-containing flame-retardant N-phenylmaleimide, instead of adding a large molecular weight "phosphorus" flame retardant, a small molecular weight allyl dioctyl phosphate is added in an amount of 400 g. That is, first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 5 times, and 3000 g of cyclohexane, 1000 g of N-phenylmaleimide, 400 g of allyl dioctyl phosphate, and 3.0 g of tert-dodecyl mercaptan are added to the polymerization reactor in sequence, and the mixture is stirred and heated. When the temperature of the polymerization reactor reaches 80°C, 1.0 g of DCP is added and the mixture is reacted for 3.0 hours. Then, 30 g of ethanol is added to terminate the reaction. The mixture is filtered, washed, purified, and dried to obtain phosphorus-containing flame-retardant N-phenylmaleimide-5.
[0164] The phosphorus-containing flame-retardant N-phenylmaleimide-5 obtained in this comparative example has an Mn of 37,000 and an Mw / Mn of 4.69; in the general formula described in Formula I, R is an octyl group (C8H 17 ), B is 1,3-butadiene, n, m are the number of repeating units: n≥1, m≥1.
[0165] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: The difference from the present invention is that in the preparation process of environmentally friendly heat-resistant flame-retardant ABS resin, phosphorus-containing flame-retardant N-phenylmaleimide is not added, but phosphorus-containing flame-retardant N-phenylmaleimide-5 is added, and the addition amount is 600g, that is: 20000g of ABS (765) resin, 600g of phosphorus-containing flame-retardant N-phenylmaleimide, 60g of calcium stearate and 80g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 20min, and then the mixed materials are directly added to a Φ60 screw kneader, and the reaction temperatures (℃) of each section of the screw are: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed is 50rpm, extrusion, cooling, granulation, and environmentally friendly heat-resistant flame-retardant ABS resin are obtained. Sampling analysis: Standard samples are made, and the test properties are shown in Table 1.
[0166] Comparative Example 6
[0167] (1) Preparation of flame-retardant N-phenylmaleimide: The difference from the present invention is that in the preparation process of phosphorus-containing flame-retardant N-phenylmaleimide, instead of adding a large molecular weight "phosphorus" flame retardant, methyl methacrylate is added in an amount of 400 g, that is, firstly, in an 8L stainless steel reactor with a jacket, nitrogen is passed through and replaced 5 times, and 3000 g of cyclohexane, 1000 g of N-phenylmaleimide, 400 g of methyl methacrylate, and 3.0 g of tert-dodecyl mercaptan are added to the polymerization reactor in sequence, and the mixture is stirred and heated. When the temperature of the polymerization reactor reaches 80°C, 1.0 g of DCP is added and reacted for 3.0 hours, and then 30 g of ethanol is added to terminate the reaction. The mixture is filtered, washed, purified, and dried to obtain flame-retardant N-phenylmaleimide.
[0168] The flame-retardant N-phenylmaleimide obtained in this comparative example has an Mn of 33,000 and an Mw / Mn of 4.32; in the general formula described in Formula I, R is methyl (CH3), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0169] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: The difference from the present invention is that in the preparation process of environmentally friendly heat-resistant flame-retardant ABS resin, phosphorus-containing flame-retardant N-phenylmaleimide is not added, but flame-retardant N-phenylmaleimide is added in an amount of 600g, that is, 20000g of ABS (765) resin, 600g of phosphorus-containing flame-retardant N-phenylmaleimide, 60g of calcium stearate and 80g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 20min, and then the mixed materials are directly added to a Φ60 screw kneader, and the reaction temperatures (℃) of each section of the screw are: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed is 50rpm, extrusion, cooling, granulation, and environmentally friendly heat-resistant flame-retardant ABS resin are obtained. Sampling analysis: Standard samples are made, and the test properties are shown in Table 1.
[0170] Comparative Example 7
[0171] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: The difference from the present invention is that in the preparation process of phosphorus-containing flame-retardant N-phenylmaleimide, no large molecular weight "phosphorus" flame retardant is added, but N-(4-bromophenyl) maleimide is added in an amount of 400g, that is: first, in an 8L stainless steel reactor with a jacket, nitrogen is replaced 5 times, 3000g of cyclohexane, 1000g of N-phenylmaleimide, 400g of N-(4-bromophenyl) maleimide, and 3.0g of tert-dodecyl mercaptan are added to the polymerization reactor in sequence, stirred and mixed, heated, and when the polymerization reactor temperature reaches 80°C, 1.0g of DCP is added and reacted for 3.0hr, and then 30g of ethanol is added to terminate the reaction, and the flame-retardant N-phenylmaleimide is obtained after suction filtration, washing, purification and drying. The flame-retardant N-phenylmaleimide a obtained in this comparative example is obtained.
[0172] The phosphorus-containing flame-retardant N-phenylmaleimide a obtained in this embodiment has an Mn of 36,000 and an Mw / Mn of 4.46; in the general formula described in Formula I, R is a bromine atom (Br), B is 1,3-butadiene, and n and m are the number of repeating units: n≥1, m≥1.
[0173] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: The difference from the present invention is that in the preparation process of environmentally friendly heat-resistant flame-retardant ABS resin, phosphorus-containing flame-retardant N-phenylmaleimide is not added, but flame-retardant N-phenylmaleimide a is added, and the addition amount is 600g, that is, 20000g of ABS (765) resin, 600g of flame-retardant N-phenylmaleimide a, 60g of calcium stearate and 80g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 20min, and then the mixed materials are directly added to a Φ60 screw kneader, and the reaction temperatures (℃) of each section of the screw are: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed is 50rpm, extrusion, cooling, granulation, and environmentally friendly heat-resistant flame-retardant ABS resin are obtained. Sampling analysis: Standard samples are prepared, and the test properties are shown in Table 1.
[0174] Comparative Example 8
[0175] (1) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide:
[0176] a. Preparation of macromolecular "phosphorus" flame retardant: same as Example 6.
[0177] b. Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: same as Example 6.
[0178] (2) Preparation of environmentally friendly heat-resistant flame-retardant ABS resin: Other conditions are similar to those in Example 6, except that the amount of phosphorus-containing flame-retardant N-phenylmaleimide added during the preparation of environmentally friendly heat-resistant flame-retardant ABS resin is 100 g, that is, 20,000 g of ABS (765) resin, 100 g of phosphorus-containing flame-retardant N-phenylmaleimide, 60 g of calcium stearate and 80 g of antioxidant 1076 are added to a high-speed mixer and mixed at high speed for 20 min, and then the mixed materials are directly added to a Φ60 screw kneader, and the reaction temperatures (°C) of each section of the screw are: 180, 180, 190, 190, 200, 210, 195, 185, 180; the screw speed is 50 rpm, extrusion, cooling, and granulation are performed to obtain environmentally friendly heat-resistant flame-retardant ABS resin. Sampling analysis: Standard samples are prepared, and the test properties are shown in Table 1.
[0179] Table 1 Properties of environmentally friendly heat-resistant and flame-retardant ABS resin
[0180]
[0181] Reference Sample * : The self-test value of commercially available ABS resin (765) produced by Daqing Petrochemical Company of China National Petroleum Corporation.
[0182] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A phosphorus-containing flame-retardant N-phenylmaleimide, characterized in that The structural formula is any of the following: n, m are the number of repeating units, and n≥1, m≥1; The number average molecular weight of the phosphorus-containing flame-retardant N-phenylmaleimide is 20,000 to 50,000, and the ratio of the weight average molecular weight to the number average molecular weight is 3.43 to 4.
12.
2. The method for preparing the phosphorus-containing flame-retardant N-phenylmaleimide according to claim 1, characterized in that The following steps are involved: (1) Preparation of macromolecular phosphorus flame retardants: Under the protection of inert gas, a first raw material system is added to solvent I, and a first polymerization initiator is added after the temperature is raised to 60-70° C., and the reaction is carried out at 60-70° C. for 180-240 minutes to obtain a first block system; then a second raw material system is added to the first block system, and the temperature is raised to 75-85° C. for 80-100 minutes, and 1,3-butadiene is added for end-capping, and the macromolecular phosphorus flame retardant is obtained after washing and drying; The first polymerization initiator is a hydrocarbyl monolithium compound; The first raw material system is composed of allyl phosphate diester and structure regulator I, and the mass ratio of allyl phosphate diester to structure regulator I is 100: (0.7-0.9); 5.7-11.4 mmol of the first polymerization initiator is used for every 1000 g of allyl phosphate diester; The second raw material system consists of styrene and structure regulator II; The mass ratio of the allyl phosphate diester to styrene and structure regulator II in the second raw material system is 100:(10-20):(0.2-0.4); The mass ratio of the allyl phosphate diester to the 1,3-butadiene is 100:(1-3); The structure regulator I and the structure regulator II are both polar organic compounds, and the structure regulator I and the structure regulator II are the same polar organic compound; (2) Preparation of phosphorus-containing flame-retardant N-phenylmaleimide: Under the protection of inert gas, N-phenylmaleimide, a molecular weight regulator and the macromolecular phosphorus flame retardant obtained in step (1) are added to solvent II, and a second polymerization initiator is added when heated to 70-80° C. to react for 120-180 minutes, and then a terminator is added to terminate the reaction, and the phosphorus-containing flame-retardant N-phenylmaleimide is obtained after suction filtration, washing, purification and drying; The second polymerization initiator is an organic peroxide; The mass ratio of the N-phenylmaleimide, the molecular weight regulator, the macromolecular phosphorus flame retardant, and the second polymerization initiator is 100:(0.1-0.3):(30-40):(0.05-0.1).
3. The method for preparing the phosphorus-containing flame-retardant N-phenylmaleimide according to claim 2, characterized in that In the step (1): The allyl phosphate diester is any one of dimethyl allyl phosphate, diethyl allyl phosphate, dipropyl allyl phosphate, dibutyl allyl phosphate, dipentyl allyl phosphate, dihexyl allyl phosphate, diheptyl allyl phosphate or dioctyl allyl phosphate; The first polymerization initiator is any one of n-butyl lithium, sec-butyl lithium, methylbutyl lithium, phenylbutyl lithium, naphthalene lithium, cyclohexyl lithium, and dodecyl lithium; The structure regulator I and the structure regulator II are any one of diethylene glycol dimethyl ether, tetrahydrofuran, ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether and triethylamine.
4. The method for preparing the phosphorus-containing flame-retardant N-phenylmaleimide according to claim 3, characterized in that In the step (2): The second polymerization initiator is any one of dicumyl peroxide, cumyl hydroperoxide, benzoyl peroxide or di-tert-butyl peroxide; The molecular weight regulator is any one of tert-decyl mercaptan, tert-dodecyl mercaptan, tert-tetradecyl mercaptan and tert-hexadecyl mercaptan.
5. The method for preparing the phosphorus-containing flame-retardant N-phenylmaleimide according to claim 4, characterized in that In the step (2): The terminator is any one of methanol, ethanol, propanol or butanol, and the mass ratio of the terminator to N-phenylmaleimide is (1-3):
100.
6. The method for preparing the phosphorus-containing flame-retardant N-phenylmaleimide according to any one of claims 2 to 5, characterized in that: The solvent I in step (1) and the solvent II in step (2) are both hydrocarbon solvents, selected from any one of pentane, hexane, octane, heptane, cyclohexane, benzene, toluene, xylene or ethylbenzene; The mass ratio of solvent I to the allyl phosphate diester is (2-3):1; The mass ratio of solvent II to the N-phenylmaleimide is (2-3): 1; And solvent I and solvent II are selected from the same hydrocarbon solvent.
7. A method for preparing an environmentally friendly heat-resistant and flame-retardant ABS resin, characterized in that The following steps are involved: Fully mix ABS resin, the phosphorus-containing flame-retardant N-phenylmaleimide according to claim 1, a stabilizer and an antioxidant in a mixer; the mass ratio of the ABS resin, the phosphorus-containing flame-retardant N-phenylmaleimide, the stabilizer and the antioxidant is 100:(1-3):(0.1-0.3):(0.2-0.4); The mixed materials are added into a screw kneader, and are subjected to reaction extrusion, cooling and granulation to obtain an environmentally friendly heat-resistant and flame-retardant ABS resin.
8. The method for preparing the environmentally friendly heat-resistant and flame-retardant ABS resin according to claim 7, characterized in that: ABS resin is a terpolymer composed of styrene, acrylonitrile and 1,3-butadiene; The stabilizer is stearate; The antioxidant is antioxidant 1076.
9. The method for preparing the environmentally friendly heat-resistant and flame-retardant ABS resin according to claim 8, characterized in that: The temperature of the reaction extrusion is 180-210° C., and the screw speed is 30-50 rpm; the screw kneading machine is a single-screw extruder or a multi-screw extruder.