Formula of self-lubricating hydrogenated butadiene-acrylonitrile rubber double-lip seal

By adding mixed wax and anti-aging agents to hydrogenated nitrile rubber double-lip sealing products, the installation difficulties caused by high roughness of the installation site are solved, the wear resistance and service life are improved, the installation process is simplified, and the labor is reduced cost.

CN118909333APending Publication Date: 2024-11-08HENGSHUI CHUANGCHENG SEALING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411319286.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The surface roughness of the installation parts of existing hydrogenated nitrile rubber double-lip sealing products is high, which leads to greater resistance during installation, increasing labor intensity and labor costs.

Method used

The formula of hydrogenated nitrile rubber main material, reinforcement and lubricant is used, where mixed wax is added as lubricant, and a dense protective film is precipitated from the rubber through mixing and vulcanization, improving wear resistance and lubricity, and at the same time, it adds anti-aging and flame retardants to extend service life.

Benefits of technology

It significantly reduces installation difficulty and labor costs, extends the service life of double-lip seals, improves the wear resistance and lubricity of rubber, and simplifies the installation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909333A_ABST
    Figure CN118909333A_ABST
Patent Text Reader

Abstract

The invention relates to the field of hydrogenated butadiene-acrylonitrile rubber, in particular to a formula of a self-lubricating hydrogenated butadiene-acrylonitrile rubber double-lip seal. According to the technical scheme, the formula of the self-lubricating hydrogenated butadiene-acrylonitrile rubber double-lip seal comprises a hydrogenated butadiene-acrylonitrile rubber main material, a reinforcing agent and a lubricating agent, and the lubricating agent is prepared from microcrystal wax, polyester wax, polyethylene wax and petroleum wax; compared with a double-lip sealing product made by an existing hydrogenated butadiene-acrylonitrile rubber formula, the hydrogenated butadiene-acrylonitrile rubber formula has the advantages that the surface roughness of a mounting part is relatively large, so that relatively large resistance needs to be overcome during mounting, the mounting efficiency is reduced for a long time, and the labor cost is increased; and through mixing and vulcanization, a compact and smooth protective film is continuously separated out from the hydrogenated nitrile rubber, so that the wear resistance and the lubricity of the rubber are improved, the service life of the double-lip seal is prolonged, and the mounting process is simpler and easier to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of hydrogenated nitrile rubber, in particular to a formula of a self-lubricating hydrogenated nitrile rubber double-lip seal. Background Art

[0002] Hydrogenated nitrile rubber is a highly saturated elastomer obtained by special hydrogenation of nitrile rubber. Hydrogenated nitrile rubber has good oil resistance (good resistance to fuel oil, lubricating oil and aromatic solvents), and due to its highly saturated structure, it has good heat resistance, excellent chemical corrosion resistance (good resistance to Freon, acid and alkali), excellent ozone resistance, high compression set resistance, and high strength, high tear resistance, excellent wear resistance, etc. It is one of the rubbers with outstanding comprehensive performance and is widely used in the manufacture of various oil-resistant rubber products. Among them, the double-lip seal made of hydrogenated nitrile rubber as raw material has attracted much attention; the surface roughness of the installation part of the double-lip seal products made of the existing hydrogenated nitrile rubber formula is relatively large, resulting in the need to overcome greater resistance when installing the double-lip seal products, which increases the labor intensity during the installation process, reduces the installation efficiency in the long run, and thus increases the labor cost. Summary of the invention

[0003] In order to overcome the problem that the surface roughness of the installation part of the double-lip seal products made of the existing hydrogenated nitrile rubber formula is relatively large, it is necessary to overcome greater resistance when installing the double-lip seal products, which increases the labor intensity during the installation process, reduces the installation efficiency in the long run, and thus increases the labor cost.

[0004] The technical solution of the present invention is: a formula of a self-lubricating hydrogenated nitrile rubber double-lip seal, comprising a hydrogenated nitrile rubber main material, a reinforcing agent and a lubricant, wherein the weight proportion of the hydrogenated nitrile rubber main material is 70-90 parts, the weight proportion of the reinforcing agent is 1-5 parts, and the weight proportion of the lubricant is 8-13 parts.

[0005] Preferably, compared with the double-lip seal products made from the existing hydrogenated nitrile rubber formula, the surface roughness of the installation part is relatively large, which increases the labor intensity during the installation process, reduces the installation efficiency in the long run, and thus increases the labor cost. The formula of the hydrogenated nitrile rubber adds mixed wax as a lubricant, and through mixing and vulcanization, a dense and smooth protective film is continuously precipitated from the hydrogenated nitrile rubber, thereby improving the wear resistance and lubricity of the rubber itself, which not only extends the service life of the double-lip seal, but also makes the installation process simpler and easier to operate.

[0006] Preferably, the lubricant consists of the following components: microcrystalline wax, polyester wax, polyethylene wax and petroleum wax, wherein the mass proportion of each component in the lubricant is: microcrystalline wax 17%, polyester wax 37%, polyethylene wax 42%, and petroleum wax 4%.

[0007] Preferably, the lubricant is obtained by the following process: S11: Perform preliminary preparations and weigh the raw materials of microcrystalline wax, polyester wax, polyethylene wax and petroleum wax respectively; S12: heating the microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials respectively to melt the microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials; S13: mixing the melted microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials and stirring them, wherein the stirring speed is set to 100 revolutions per minute and the stirring time is 25 minutes; S14: After the stirring is completed, the mixture is rapidly cooled to 20 degrees Celsius.

[0008] Preferably, a vulcanizing agent is also included, and the weight proportion of the vulcanizing agent is 1 part to 3 parts, wherein the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0009] Preferably, an antioxidant is also included, and the weight proportion of the antioxidant is 0.5 to 2 parts, wherein the antioxidant is 4,4′-bis(α,α′-dimethylbenzyl)diphenylamine.

[0010] Preferably, by using 4,4′-bis(α,α′-dimethylbenzyl)diphenylamine, that is, antioxidant RD, as the antioxidant, antioxidant RD effectively prolongs the service life of rubber products through its multiple effects such as anti-oxidation, anti-ozone, anti-heat aging and anti-hydrolysis. It can prevent the rubber products from hardening and cracking due to aging, and maintain their original elasticity and softness. Anti-aging agent RD has good solubility in rubber and can be evenly dispersed during the rubber processing process, thereby improving the mixing effect and facilitating processing.

[0011] Preferably, a flame retardant is also included, and the weight proportion of the flame retardant is 0.5 parts to 2.5 parts, wherein the flame retardant is one of a halogen flame retardant, a phosphorus flame retardant, a nitrogen flame retardant and an inorganic flame retardant.

[0012] Preferably, a softener is also included, and the weight proportion of the softener is 5 to 8 parts, wherein the softener is one of dioctyl phthalate and dibutyl phthalate.

[0013] Preferably, the reinforcing agent is silicon dioxide, wherein the silicon dioxide is silicon dioxide modified by γ-mercaptopropyltrimethoxysilane.

[0014] Preferably, when the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener are mixed, the following steps are included: S21: Raw material preparation, weighing the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener according to the proportion; S22: preheating the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener respectively; S23: stirring and mixing the preheated hydrogenated nitrile rubber main material and the lubricant, with the stirring speed set to 150 revolutions per minute and the stirring time set to 30 minutes; S24: adding a reinforcing agent, a vulcanizing agent, an antioxidant, a flame retardant and a softener, and continuing to stir, the stirring time is set to 40 minutes, and the stirring speed is set to 90 revolutions per minute; S25: After the mixing is completed, the mixture is rapidly cooled to 20 degrees Celsius.

[0015] Preferably, when preheating the hydrogenated nitrile rubber main material, the preheating temperature is 45 degrees Celsius.

[0016] Preferably, by adding a reinforcing agent to the formula of hydrogenated nitrile rubber, the tensile strength, elongation at break and tear strength of the rubber can be significantly improved, while its heat resistance and aging resistance can be improved, and its wear resistance can be further improved. At the same time, by adding one of dioctyl phthalate and dibutyl phthalate as a softener to the formula of hydrogenated nitrile rubber, the processing performance and softness of the hydrogenated nitrile rubber can be improved, thereby improving the use performance of the hydrogenated nitrile rubber.

[0017] Beneficial effects of the present invention: 1. Compared with the double-lip seal products made of existing hydrogenated nitrile rubber formula, the surface roughness of the installation part is relatively large, resulting in the need to overcome greater resistance when installing the double-lip seal products, which increases the labor intensity during the installation process, reduces the installation efficiency in the long run, and thus increases the labor cost. The formula of hydrogenated nitrile rubber adds mixed wax as a lubricant, and through mixing and vulcanization, a dense and smooth protective film is continuously precipitated from the hydrogenated nitrile rubber, thereby improving the wear resistance and lubricity of the rubber itself, which not only extends the service life of the double-lip seal, but also makes the installation process simpler and easier to operate; 2. By using 4,4′-bis(α,α′-dimethylbenzyl)diphenylamine, antioxidant RD, as an antioxidant, antioxidant RD effectively extends the service life of rubber products through its multiple functions such as anti-oxidation, anti-ozone, anti-heat aging and anti-hydrolysis. It can prevent rubber products from hardening and cracking due to aging, and maintain their original elasticity and softness. Antioxidant RD has good solubility in rubber and can be evenly dispersed during the rubber processing process, thereby improving the mixing effect and facilitating processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Shown is a schematic diagram of the processing flow of the lubricant in the formula of the self-lubricating hydrogenated nitrile rubber double-lip seal of the present invention; Figure 2 Shown is a schematic diagram of the processing flow in the formulation of the self-lubricating hydrogenated nitrile rubber double lip seal of the present invention. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0020] See also Figure 1-2 The present invention provides an embodiment: a formula for a self-lubricating hydrogenated nitrile rubber double-lip seal, comprising a hydrogenated nitrile rubber main material, a reinforcing agent and a lubricant, wherein the weight proportion of the hydrogenated nitrile rubber main material is 70-90 parts, the weight proportion of the reinforcing agent is 1-5 parts, and the weight proportion of the lubricant is 8-13 parts.

[0021] Preferably, compared with the double-lip seal products made from the existing hydrogenated nitrile rubber formula, the surface roughness of the installation part is relatively large, resulting in the need to overcome greater resistance when installing the double-lip seal products, which increases the labor intensity during the installation process, reduces the installation efficiency in the long run, and thus increases the labor cost. The hydrogenated nitrile rubber formula adds mixed wax as a lubricant, and through mixing and vulcanization, a dense and smooth protective film is continuously precipitated from the hydrogenated nitrile rubber, thereby improving the wear resistance and lubricity of the rubber itself, which not only extends the service life of the double-lip seal, but also makes the installation process simpler and easier to operate.

[0022] Preferably, the lubricant consists of the following components: microcrystalline wax, polyester wax, polyethylene wax and petroleum wax, wherein the mass proportion of each component in the lubricant is: microcrystalline wax 17%, polyester wax 37%, polyethylene wax 42%, and petroleum wax 4%.

[0023] Preferably, the lubricant is obtained by the following process: S11: Perform preliminary preparations and weigh the raw materials of microcrystalline wax, polyester wax, polyethylene wax and petroleum wax respectively; S12: heating the microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials respectively to melt the microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials; S13: mixing the melted microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials and stirring them, wherein the stirring speed is set to 100 revolutions per minute and the stirring time is 25 minutes; S14: After the stirring is completed, the mixture is rapidly cooled to 20 degrees Celsius.

[0024] Preferably, a vulcanizing agent is also included, and the weight proportion of the vulcanizing agent is 1 part to 3 parts, wherein the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0025] Preferably, an antioxidant is also included, and the weight proportion of the antioxidant is 0.5 to 2 parts, wherein the antioxidant is 4,4′-bis(α,α′-dimethylbenzyl)diphenylamine.

[0026] Preferably, by using 4,4′-bis(α,α′-dimethylbenzyl)diphenylamine, that is, antioxidant RD, as the antioxidant, antioxidant RD effectively prolongs the service life of rubber products through its multiple effects such as anti-oxidation, anti-ozone, anti-heat aging and anti-hydrolysis. It can prevent the rubber products from hardening and cracking due to aging, and maintain their original elasticity and softness. Anti-aging agent RD has good solubility in rubber and can be evenly dispersed during the rubber processing process, thereby improving the mixing effect and facilitating processing.

[0027] Preferably, a flame retardant is also included, and the weight proportion of the flame retardant is 0.5 parts to 2.5 parts, wherein the flame retardant is one of a halogen flame retardant, a phosphorus flame retardant, a nitrogen flame retardant and an inorganic flame retardant.

[0028] Preferably, a softener is also included, and the weight proportion of the softener is 5 to 8 parts, wherein the softener is one of dioctyl phthalate and dibutyl phthalate.

[0029] Preferably, the reinforcing agent is silicon dioxide, wherein the silicon dioxide is silicon dioxide modified by γ-mercaptopropyltrimethoxysilane.

[0030] Preferably, when the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener are mixed, the following steps are included: S21: Raw material preparation, weighing the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener according to the proportion; S22: preheating the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener respectively; S23: stirring and mixing the preheated hydrogenated nitrile rubber main material and the lubricant, with the stirring speed set to 150 revolutions per minute and the stirring time set to 30 minutes; S24: adding a reinforcing agent, a vulcanizing agent, an antioxidant, a flame retardant and a softener, and continuing to stir, the stirring time is set to 40 minutes, and the stirring speed is set to 90 revolutions per minute; S25: After the mixing is completed, the mixture is rapidly cooled to 20 degrees Celsius.

[0031] Preferably, when preheating the hydrogenated nitrile rubber main material, the preheating temperature is 45 degrees Celsius.

[0032] Preferably, by adding a reinforcing agent to the formula of hydrogenated nitrile rubber, the tensile strength, elongation at break and tear strength of the rubber can be significantly improved, while its heat resistance and aging resistance can be improved, and its wear resistance can be further improved. At the same time, by adding one of dioctyl phthalate and dibutyl phthalate as a softener to the formula of hydrogenated nitrile rubber, the processing performance and softness of the hydrogenated nitrile rubber can be improved, thereby improving the use performance of the hydrogenated nitrile rubber.

[0033] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of those skilled in the art without departing from the spirit of the present invention.

Claims

1. A formula for a self-lubricating hydrogenated nitrile rubber double lip seal; characterized in that: The invention comprises a hydrogenated nitrile rubber main material, a reinforcing agent and a lubricant, wherein the weight proportion of the hydrogenated nitrile rubber main material is 70-90 parts, the weight proportion of the reinforcing agent is 1-5 parts, and the weight proportion of the lubricant is 8-13 parts.

2. The formula of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 1, characterized in that: The lubricant is composed of the following ingredients: microcrystalline wax, polyester wax, polyethylene wax and petroleum wax, among which the mass proportion of each ingredient in the lubricant is: microcrystalline wax 17%, polyester wax 37%, polyethylene wax 42%, and petroleum wax 4%.

3. The formula of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 2, characterized in that: The lubricant is obtained by: S11: Perform preliminary preparations and weigh the raw materials of microcrystalline wax, polyester wax, polyethylene wax and petroleum wax according to the set mass ratios; S12: heating the microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials respectively to melt the microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials; S13: mixing the melted microcrystalline wax, polyester wax, polyethylene wax and petroleum wax raw materials and stirring them, wherein the stirring speed is set to 100 revolutions per minute and the stirring time is 25 minutes; S14: After the stirring is completed, the mixture is rapidly cooled to 20 degrees Celsius.

4. The formula of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 3, characterized in that: The invention also includes a vulcanizing agent, the weight proportion of the vulcanizing agent is 1 part to 3 parts, wherein the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

5. The formula of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 4, characterized in that: The invention also comprises an antioxidant, the weight proportion of which is 0.5 to 2 parts, wherein the antioxidant is 4,4′-bis(α,α′-dimethylbenzyl)diphenylamine.

6. The formula of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 5, characterized in that: The invention also comprises a flame retardant, the weight proportion of the flame retardant is 0.5-2.5 parts, wherein the flame retardant is one of a halogen flame retardant, a phosphorus flame retardant, a nitrogen flame retardant and an inorganic flame retardant.

7. A formulation of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 6, characterized in that: The invention also comprises a softener, the weight proportion of the softener is 5 to 8 parts, wherein the softener is one of dioctyl phthalate and dibutyl phthalate.

8. The formula of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 7, characterized in that: The reinforcing agent is silicon dioxide, wherein the silicon dioxide is silicon dioxide modified by gamma-mercaptopropyltrimethoxysilane.

9. A formulation for a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 8, characterized in that: When the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener are mixed, the following steps are included: S21: Raw material preparation, weighing the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener according to the proportion; S22: preheating the hydrogenated nitrile rubber main material, reinforcing agent, lubricant, vulcanizing agent, antioxidant, flame retardant and softener respectively; S23: stirring and mixing the preheated hydrogenated nitrile rubber main material and the lubricant, with the stirring speed set to 150 revolutions per minute and the stirring time set to 30 minutes; S24: adding a reinforcing agent, a vulcanizing agent, an antioxidant, a flame retardant and a softener, and continuing to stir, the stirring time is set to 40 minutes, and the stirring speed is set to 90 revolutions per minute; S25: After the mixing is completed, the mixture is rapidly cooled to 20 degrees Celsius.

10. The formula of a self-lubricating hydrogenated nitrile rubber double lip seal according to claim 9, characterized in that: When preheating the hydrogenated nitrile rubber main material, the preheating temperature is 45 degrees Celsius.