Laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device and process thereof
Through laser thermal softening assisted ultrasonic rolling technology, the problem of unsatisfactory surface strengthening effect of high-temperature alloys is solved, deep plastic deformation and fatigue resistance are improved, tool wear is reduced, and processing efficiency and surface quality are improved.
Patent Information
- Application Number
- CN202410949650.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-15
AI Technical Summary
When strengthening high-temperature alloys, the strengthening effect is not ideal, the surface hardened layer has shallow depth, severe microcracks, and severe tool wear, making it difficult to achieve ideal fatigue resistance.
The laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device is used to thermally soften the workpiece surface through a laser, and strengthen it with an ultrasonic rolling tool to achieve deep plastic deformation of the material and improve the microstructure and reduce tool wear.
It significantly improves the hardness and fatigue resistance of the material surface reinforcement layer, reduces surface defects, extends tool life, and achieves an efficient processing process.
Smart Images

Figure CN118957209A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material surface strengthening, and specifically relates to a laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device and a process thereof. Background Art
[0002] Due to their high specific strength and excellent high-temperature oxidation resistance and fatigue resistance, difficult-to-process materials such as high-temperature alloys are increasingly needed in the manufacture and use of key aero-engine structural parts. The service environment of these structural parts is usually under extremely harsh conditions. Wear, fatigue cracks and fractures are the main failure forms of key aero-engine structural parts such as drive shafts, turbine blades, and turbine disks during their service. More than 80% of fatigue failures of aero-engine structural parts occur on the surface and sub-surface of components. It can be seen that the surface quality of components is the main cause of component failure. In order to avoid fatigue failure of various components and parts, it is urgent to introduce surface strengthening technology on the basis of anti-fatigue cutting / grinding technology to improve the surface structure and stress state in order to improve its fatigue performance and the service life of components.
[0003] At present, the most representative traditional surface strengthening technologies are shot peening and rolling strengthening, which mainly improve the fatigue performance of materials by introducing residual compressive stress in the surface layer, increasing the microhardness, and inducing the refinement of the microstructure of the surface material. However, due to the randomness of shot peening and the difficulty in accurately controlling the shot peening area and intensity, shot peening technology is prone to cause surface defects such as delamination and wrinkles, which have an adverse effect on the fatigue performance of the strengthened workpiece; in addition, shot peening can cause shot splashing and contamination, and the projectiles need to be recovered; and rolling strengthening will generate greater friction in the contact area between the rolling tool and the workpiece surface during processing, causing shear stress on the subsurface of the workpiece and scratching the workpiece surface, which is not conducive to improving the fatigue strength of the parts. Therefore, the surface performance and fatigue performance of the workpiece after using only a single traditional mechanical surface strengthening technology still cannot meet the requirements, and the strengthening effect is limited.
[0004] However, with the rapid development of domestic aerospace and other fields and material technology, higher requirements have been put forward for the performance of various aspects of aero-engine parts, and some new surface strengthening technologies have emerged, such as laser shot peening, ultrasonic impact, ultrasonic shot peening and ultrasonic rolling, which have achieved good results in improving the fatigue resistance and wear resistance of parts. Compared with the above-mentioned surface strengthening technologies, ultrasonic rolling strengthening technology has overcome the defects of traditional processes such as shot peening and rolling to varying degrees, breaking through the limitation that traditional single mechanical processing technology cannot simultaneously achieve shape control and controllability. It can obtain lower surface roughness and friction coefficient on the surface of the workpiece material, give the surface a higher microhardness, introduce deeper and more uniform residual compressive stress, significantly improve the service performance of the specimen, and effectively slow down the surface wear failure of the material. More importantly, no chips are generated during the rolling process, its principle and operation are simple, the processing efficiency is high, the cost is low, and low energy consumption, low pollution and low emission production can be achieved. It is a green and efficient surface engineering technology that helps achieve the "dual carbon" goal, with important practical value and broad application prospects. However, the strengthening effect of ultrasonic rolling technology depends on the characteristics of the material itself. Based on the low plasticity and high strength characteristics of GH4169 high-temperature alloy, it is very difficult to produce strong plastic deformation when using this technology to strengthen GH4169 high-temperature alloy. The depth of the formed surface hardening layer and residual compressive stress layer is very shallow, and the strengthening effect is not very ideal; secondly, the micro-hardness distribution gradient of the surface strengthening layer after rolling is large, and the work hardening phenomenon is serious. The surface of the material is prone to microcracks and poor surface quality, which seriously affects the service life of the structural parts. In addition, the ultrasonic rolling head of the existing device cannot be disassembled and replaced, and it is easy to cause the tool head to wear or even fall off after long-term use. Therefore, it is impossible to achieve the ideal strengthening effect by relying solely on ultrasonic rolling technology. It is urgent to seek a more complete and practical ultrasonic rolling surface strengthening device and its operation process to achieve efficient strengthening treatment of high-temperature alloys.
[0005] Many studies have shown that the temperature distribution of the material surface and shallow surface layer plays a vital role in ultrasonic rolling, and has a great influence on the stress, strength and hardness of material deformation. It determines the thermal softening depth of the material and is also a key factor in whether ultrasonic rolling can proceed smoothly and obtain a better surface strengthening layer. At present, there are many ways to apply temperature heat source based on ultrasonic rolling strengthening technology, such as pulse electromagnetic coupling auxiliary technology, thermal field auxiliary technology, laser auxiliary technology, etc.
[0006] The invention patent with the authorization announcement number CN114836605B by Ye Chang and others from Huazhong University of Science and Technology discloses a pulsed electric field and magnetic field assisted ultrasonic rolling strengthening device and method. This patent mainly promotes the refinement of workpiece grains through the coupling of multiple physical fields such as pulsed electric field and pulsed magnetic field, so as to significantly improve the thickness of the strengthening layer and fatigue performance of the material. However, this patent wraps the coil around the metal workpiece processing area to apply the magnetic field, and the action area of the magnetic field is limited to the range of the wound coil, which limits the strengthening area of ultrasonic rolling. At the same time, the pulse discharge electrode is set in the workpiece processing area, which will form a large heat-affected zone, causing large-area heating of the workpiece, resulting in thermal deformation, and the pretreatment operation is cumbersome.
[0007] The invention patent with authorization announcement number CN112877517B by Li Yugang and others from Shanghai Jiao Tong University discloses a surface strengthening device and method for applying a thermal field to a metal workpiece and assisting ultrasonic rolling. A heater is used to apply a thermal field to the strengthened metal workpiece material. On this basis, a temperature monitor connected to a feedback regulation controller is used to monitor the surface temperature of the workpiece, thereby realizing dynamic heating during the ultrasonic rolling strengthening process, thereby improving the mechanical properties of the metal material, appropriately reducing the plastic deformation resistance of the surface layer of the workpiece to be strengthened, and making the residual compressive stress level and layer depth of the surface strengthening layer of the material higher. Compared with the single ultrasonic rolling strengthening technology, the thickness of the workpiece surface strengthening layer is further deepened, and the microhardness is further improved, which effectively improves the ultrasonic rolling strengthening efficiency and strengthening effect, but the temperature applied by the thermal field is not easy to control.
[0008] The invention patent with authorization announcement number CN115922231B by Zhao Jian et al. of Taiyuan University of Technology discloses a rotary ultrasonic rolling device integrating laser softening and strengthening technology. This patent mainly uses laser to pre-treat the workpiece with heat softening, and then uses an ultrasonic rolling tool to roll and strengthen the same position on the surface of the workpiece that has been pre-treated by laser. Although a better strengthening effect is achieved during processing, the laser heat on the surface of the workpiece is gradually dissipated at this time, resulting in a large temperature gradient inside the material, which will cause large thermal stress inside the material. When the thermal stress exceeds the yield strength of the material, cracks will appear inside the material, making the fatigue performance of the workpiece after laser-assisted ultrasonic rolling still relatively poor. The reason is that the existing device cannot achieve simultaneous strengthening of laser-assisted and ultrasonic rolling.
[0009] In summary, the thermal softening effect of temperature heat source can effectively improve the mechanical properties of difficult-to-process materials with high strength and low plasticity. Not only can better plasticity be obtained, but also beneficial microstructural changes can be produced. Combined with the joint effect of ultrasonic rolling coupling, the problem of unclear strengthening effect of single field and specific double field coupling on metal workpieces can be solved. However, when performing heat softening-assisted processing, an upper and lower limit of temperature must be given in combination with the melting point of the material, that is, there is a threshold value for the temperature heat source. Too high a temperature will not only cause residual compressive stress and work-hardened layer to be easily thermally relaxed, but also cause surface defects such as overburning and melting on the workpiece material surface, accompanied by the formation of a large amount of oxidized adhesives, and cause severe thermal wear of the tool, thereby reducing the quality of the workpiece's processed surface and the tool life. Too low a temperature will affect the role of auxiliary heating, and the thermal softening effect of the material is not obvious. Compared with other heat sources, laser has the advantages of good controllability, small spot size, and high power density. By precisely controlling the temperature of the workpiece surface, large-area heating of the entire workpiece is avoided, thermal softening of the workpiece surface is achieved, the material deformation mechanism is regulated, a deeper plastic deformation layer is induced, and the heating softening depth can be basically consistent with the cutting depth. It is the preferred heat source for research on heat softening-assisted ultrasonic rolling of GH4169 high-temperature alloy. Summary of the invention
[0010] In view of the problems and shortcomings in the above-mentioned existing difficult-to-process material surface strengthening technology, the purpose of the present invention is to provide a laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device and its process. The device has a simple structure and is easy to operate. It focuses the laser beam on the surface of the workpiece material in front of the ultrasonic rolling tool, so that the material is thermally softened while the ultrasonic rolling tool is used for strengthening. The role of the laser is to thermally soften the workpiece material, thereby improving the plasticity of the material, causing the yield strength of the material to be reduced to below the fracture strength, reducing the rolling force, slowing down the wear of the tool, and inhibiting the surface of the strengthened workpiece from cracking, falling off or cracking, thereby achieving the surface strengthening effect of the enhanced material, obtaining a better surface strengthening layer, improving the service performance of the structural parts, and solving the problems of severe wear of the rolling head, low strengthening efficiency, and low surface quality and fatigue strength during ultrasonic rolling.
[0011] To achieve the above-mentioned purpose, the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device of the present invention comprises a horizontal CNC lathe, an ultrasonic rolling assembly, a laser assembly, a temperature measuring instrument and an industrial computer, wherein: the horizontal CNC lathe mainly comprises a guide rail assembly, a three-jaw chuck, an ejector pin, a slide plate, and a tool holder; the guide rail assembly comprises a longitudinal guide rail and a transverse guide rail, wherein the transverse guide rail is arranged along the axial direction of the metal workpiece, and the longitudinal guide rail is vertically movably mounted on the transverse guide rail;
[0012] The ultrasonic rolling assembly mainly includes an ultrasonic generator, a transducer, an horn, a fixing ring and an ultrasonic rolling tool. The ultrasonic rolling tool adopts a rolling head in the form of a ball. The ultrasonic generator is placed in an integrated ultrasonic rolling device and connected to one end of the transducer inside the ultrasonic rolling assembly. The internal connection sequence is as follows: the other end of the transducer is connected to the large end of the horn, and at the same time, the small end of the horn is connected to the ultrasonic rolling head with a positioning screw. The cross section of the horn is an isosceles trapezoid, and the transducer is a cylinder, and the diameters of the connecting ends of the two are the same. In addition, the fixing ring is connected to the ultrasonic rolling fixture by bolts, and the ultrasonic frequency electrical signal is converted into ultrasonic mechanical vibration by the transducer. After being amplified by the horn, the output mechanical vibration with a certain amplitude is transmitted to the ultrasonic rolling tool and acts on the workpiece to be strengthened, and the ultrasonic rolling head is detachable. Among them, the ultrasonic frequency emitted by the transducer is in the range of 15 to 28 kHz, and the amplitude of the horn is in the range of 5 to 20 μm;
[0013] The laser assembly includes a laser controller, a laser focusing head and a support frame for fixing the laser assembly. The laser is connected to the laser focusing head via an optical fiber. The laser support frame is a "cross-shaped" structure arranged on the slide and fixed on the transverse guide rail. A 360° rotation adjustment device is provided between the laser focusing head and the support frame, and the laser incident angle and the spot diameter incident on the workpiece surface are adjusted by the 360° rotation adjustment device. The support frame with the laser focusing head is provided with a lifting adjustment device, and the support frame is lifted and moved along the y-axis by the lifting adjustment device, and the slide realizes the horizontal movement of the laser focusing head along the x-axis and z-axis through the longitudinal and transverse guide rails.
[0014] The temperature measuring instrument and the laser assembly are both connected to the industrial computer, and the industrial computer includes a computer and a host computer.
[0015] Preferably: the ultrasonic rolling head is a detachable elliptical ball with a hardness of HRC 60-92; a cooling lubrication hole is provided on the ultrasonic rolling head, and the cooling lubrication hole is connected to the integrated ultrasonic rolling device through a cooling hose laid on the outside of the ultrasonic rolling assembly, and air cooling is adopted.
[0016] Preferably: the ultrasonic rolling assembly is mounted on the tool holder, the tool holder is mounted on the other side of the slide, the slide realizes the horizontal movement of the ultrasonic rolling head along the x and z axes through the longitudinal and transverse guide rails, and in addition, the axes of the transducer, the amplitude transformer, the ultrasonic rolling head, the fixing ring and the ultrasonic rolling fixture are located on the same straight line;
[0017] According to another aspect of the present invention, the present invention also provides a process for a laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device, which specifically includes the following steps:
[0018] Step 1: Clamp the workpiece material to be strengthened on the three-jaw chuck of the horizontal CNC lathe and fix it with a thimble; in addition, fix the ultrasonic rolling assembly and the laser assembly on the tool holder and the laser support frame on both sides of the slide respectively, adjust the direction of the laser focusing head through the laser 360° rotation adjustment device, adjust the y-axis lifting movement of the laser focusing head through the lifting adjustment device, and adjust the horizontal movement of the x-axis and z-axis through the horizontal adjustment device composed of the slide and guide rail assembly, so as to achieve their coordination and make the ultrasonic rolling head contact and align with the outer circumference of the workpiece in a line contact manner;
[0019] Step 2: Turn on the laser controller and irradiate the generated laser beam through the laser focusing head to the contact area between the ultrasonic rolling and the workpiece material to be strengthened, so as to thermally soften the surface of the workpiece to be strengthened. At the same time, the industrial computer monitors the temperature T of the surface of the workpiece to be strengthened in real time through the temperature measuring instrument;
[0020] Step 3: adjusting the laser parameters according to the monitored temperature T. When the temperature T is greater than the preset laser thermal softening auxiliary temperature threshold T1, that is, T>T1, where the preset laser thermal softening auxiliary temperature threshold T1 is the melting point of the workpiece material, the laser parameters are adjusted by the laser. Under the premise of ensuring that the workpiece material is not burned, the mechanical properties of the workpiece material are changed by means of the thermal softening effect of the laser, so that the plastic deformation resistance of the surface layer of the strengthening zone is appropriately reduced, so as to achieve the purpose of laser thermal softening assisted ultrasonic rolling;
[0021] Step 4: At the same time, start the spindle, so that the three-jaw chuck drives the workpiece to rotate, and set the ultrasonic rolling parameters through the machine tool program, and realize the joint adjustment and control of the strengthening state of the laser component and the ultrasonic rolling component at the same position, so as to realize the multi-energy field synchronous coupling strengthening treatment of the workpiece. The whole operation process is realized on the horizontal CNC lathe.
[0022] Step 5: After the processing is completed, turn off the laser controller, the horizontal CNC lathe and the integrated ultrasonic rolling device, and take out the workpiece.
[0023] Furthermore, in step 1, the position of the laser focusing head is adjusted by a 360° rotating adjustment device and a lifting adjustment device on the support frame, so that the laser emitted by the laser focusing head irradiates the workpiece to be strengthened;
[0024] Preferably, in order to make the temperature distribution in the rolling area as uniform as possible, an elliptical spot is preferably selected; when the rolling depth is small and the spindle speed of the workpiece is fast, the long axis direction of the elliptical spot is adjusted to be consistent with the rotation direction of the workpiece, the laser irradiation time is increased, and the thermal softening speed is increased. When the rolling depth is large and the spindle speed of the workpiece is low, the short axis direction of the elliptical spot is adjusted to be consistent with the rotation direction of the workpiece to avoid overheating and wear of the rolling tool.
[0025] In particular, when the laser spot shape is elliptical and the laser incident angle is θ, the major semi-axis a and the minor semi-axis b of the elliptical spot are respectively:
[0026] a=r b secθ (1)
[0027] b=r b (2)
[0028] At this time, the laser power density distribution of the laser irradiating the workpiece surface should satisfy:
[0029]
[0030] Where: E is the laser beam power density at different positions on the cross section, W / m 2 ; P is laser power, W; r b is the spot radius of the laser effective area, mm; L is the circumferential distance from different positions of the cross section (rolling point) to the center of the laser spot, mm;
[0031] Empirical formula for the temperature T in the laser processing area of cylindrical bars:
[0032]
[0033] In the formula, λ is the thermal conductivity of the material, K is the diffusion coefficient, and t is the laser processing time. The temperature T of the laser processing area can be obtained by equations (3) and (4):
[0034]
[0035] Further, when the workpiece material to be strengthened in step 3 is the high temperature alloy GH4169, the preset laser thermal softening auxiliary temperature threshold T1 has a value range of 650° C. to 700° C.;
[0036] Furthermore, in step 3, the laser parameters include spot diameter D, laser power P, laser moving speed v l And the circumferential distance L between the center of the spot and the center of the ultrasonic rolling head, D is 50-80 μm, P is 6-9 W, v l 40~80m / min;
[0037] Preferably, in order to ensure that the ultrasonic rolling tool and the focused laser beam are kept in a safe range, the tool may not be damaged due to overheating due to the close distance between the ultrasonic rolling tool and the laser beam, and the workpiece surface may not be burned by the laser beam. The circumferential distance L between the center of the laser spot and the center of the ultrasonic rolling head should be controlled within the range of 0.5 to 2 mm;
[0038] In particular, the circumferential distance L between the center of the laser spot and the center of the ultrasonic rolling head can be calculated based on the angle β between the center of the ultrasonic rolling head and the center of the light beam in the cross section of the workpiece, the laser incident angle θ, and the radius R of the workpiece, and the relationship is:
[0039]
[0040] Furthermore: when performing coupled synchronous rolling strengthening in step 4, the axis of the ultrasonic rolling head should be perpendicular to the axis of the workpiece material to be strengthened, parallel to the center line of the laser spot along the circumferential direction of the workpiece to be strengthened, and the ultrasonic rolling head should be aligned with the workpiece.
[0041] Preferably, since the laser-assisted processing and ultrasonic rolling processing need to be processed synchronously, the laser moving speed v is l Should be related to the rolling speed v r The same. And the rolling depth a p and feed rate v f Should meet:
[0042] v l =v r =πDn (8)
[0043] a p =2bsinθ (9)
[0044] v f =a p tanθ=2bsinθtanθ (10)
[0045] Where: R is the workpiece radius, mm; n is the workpiece spindle speed, m / min;
[0046] Furthermore, in step 4, the ultrasonic rolling process parameters mainly include the workpiece spindle speed n, the rolling depth a p , a p 0.1~0.45mm, n is 300~650m / min;
[0047] Furthermore, in step 3 and step 4: the laser process parameters and the ultrasonic rolling parameter range are optimized and selected based on finite element simulation and laser moving speed matching thermal softening test, and the specific steps are as follows:
[0048] Step 1: Based on the heat transfer and mechanical properties of the material and the empirical formula of laser thermal softening temperature, a finite element analytical numerical model of laser thermal softening temperature field distribution is established using MATLAB software to obtain the influence of different laser process parameters on the temperature and thermal stress of the workpiece surface;
[0049] Step 2: Compare the workpiece surface temperature T under different laser process parameters with the preset laser thermal softening auxiliary temperature threshold T1, and preliminarily select the laser process parameter range in combination with the selection principle of ultrasonic rolling parameters;
[0050] Step 3: Verify and optimize the preliminary laser process parameters and ultrasonic rolling process parameter ranges through laser moving speed matching thermal softening process test.
[0051] The beneficial effects of the present invention compared to the prior art are:
[0052] (1) Realizing synchronous strengthening: The laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device and its process of the present invention realize the synchronous composite strengthening of laser thermal softening and ultrasonic rolling linkage through the coordinated cooperation of the laser 360° rotation adjustment device, the lifting adjustment device, the slide and the horizontal adjustment device composed of the longitudinal and transverse guide rails. Compared with the existing strengthening device, the thermal softening effect of the laser beam is introduced to change the mechanical properties of the workpiece material, thereby improving the plasticity of the workpiece material surface, inducing a deeper plastic deformation layer, and producing beneficial microstructural changes, realizing the regulation of the material deformation mechanism, and combining with the comprehensive effect of ultrasonic rolling synchronous coupling, the material surface modification layer has higher hardness, as well as better wear resistance and fatigue resistance, solving the problem that the strengthening effect of single field and specific double field coupling on metal workpieces is not obvious, especially some difficult-to-process materials with high hardness and low plasticity.
[0053] (2) Realizing real-time control: The strengthening device of the present invention has a simple structure. It combines an industrial computer and a temperature meter to monitor the temperature distribution in the process of laser thermal softening assisted ultrasonic rolling in real time, forming a closed-loop control, so as to adjust the laser process parameters and ultrasonic rolling process parameters in real time, ensure that the temperature in the ultrasonic rolling area is between the temperature that exceeds the softening temperature of the material and is lower than the burning temperature range of the material, avoid laser overburning, melting and rolling force overload, solve the problem of thermal stress crack defects on the surface of the workpiece, and help alleviate the overheating wear of the ultrasonic rolling tool;
[0054] (3) Achieve efficient processing: The operating process of the present invention is simple to operate and can realize multi-process operation at one workstation, saving processing time, reducing costs, and improving overall processing efficiency. In addition, the laser spot used in the present invention is elliptical, which ensures uniform temperature distribution in the rolling area and further improves the surface quality and surface performance of the strengthening layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 It is a schematic structural diagram of the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device of the present invention;
[0056] Figure 2 It is a top view schematic diagram of the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device of the present invention;
[0057] Figure 3 It is a schematic structural diagram of the ultrasonic rolling assembly 20 involved in the present invention;
[0058] Figure 4 It is a diagram of the assembly sequence of the tool holder 8 and the ultrasonic rolling assembly 20 involved in the present invention;
[0059] Figure 5 It is a structural schematic diagram of the laser assembly 13 involved in the present invention;
[0060] Figure 6 It is a schematic diagram of the geometric relationship between the laser process parameters and the ultrasonic rolling process parameters involved in the present invention;
[0061] Figure 7 This is the laser thermal softening assisted ultrasonic rolling synchronous strengthening test site and infrared temperature measurement results;
[0062] Figure 8 It is an overall framework flow chart of the preferred range of laser process parameters and ultrasonic rolling parameters involved in the present invention;
[0063] Fig. 9 This is the simulation result diagram of laser thermal softening and ultrasonic rolling thermal softening;
[0064] Fig.10 This is a comparison diagram of the SEM surface morphology and sub-surface morphology of the GH4169 high-temperature alloy material strengthened by the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device and the optimized laser assisted ultrasonic rolling composite process parameters of the present invention and the SEM surface morphology and sub-surface morphology of the material only subjected to single ultrasonic rolling;
[0065] Fig.11 A comparison chart of the three-dimensional surface morphology and cross-sectional profile curves of the GH4169 high-temperature alloy material strengthened by the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device and the optimized laser assisted ultrasonic rolling composite process parameters of the present invention and the material only subjected to single ultrasonic rolling.
[0066] Description of the main reference numerals:
[0067] 1. Horizontal CNC lathe; 2. Three-jaw chuck; 3. Ejector; 4. Slide; 5. Guide rail assembly; 6. Longitudinal guide rail; 7. Transverse guide rail; 8. Tool holder; 9. Fixer; 10. Positioning screw; 11. Clamping nut; 12. Positioning screw I; 13. Laser assembly; 14. Laser controller; 15. Laser focusing head; 16. Support frame for fixing the laser; 17. 360° rotation adjustment device; 18. Lifting adjustment device; 19. Elliptical spot; 20. Ultrasonic rolling assembly; 21. Ultrasonic rolling tool; 22. Ultrasonic rolling head; 23. Positioning screw II; 24. Cooling and lubrication hole; 25. Amplitude transformer; 26. Transducer; 27. Bolt; 28. Fixing ring; 29. Ultrasonic rolling fixture; 30. Integrated ultrasonic rolling device; 31. Thermometer; 32. Computer; 33. Computer host; 34. Workpiece to be strengthened. DETAILED DESCRIPTION
[0068] In order to make the purpose, technical solution and effect of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods so that relevant personnel can better understand and use it. It should be noted that the specific implementation described here is only used to explain the present invention and is not intended to limit the present invention.
[0069] Embodiment 1
[0070] like Figures 1-2 As shown, the present invention provides a laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device, which mainly includes an ultrasonic rolling assembly 20, a laser assembly 13, a horizontal CNC lathe 1, a temperature meter 31 and an industrial computer. Among them, the horizontal CNC lathe 1 mainly includes a three-jaw chuck 2, an ejector 3, a slide 4, a tool holder 8, and a guide rail assembly 5; the guide rail assembly 5 is arranged on the processing side of the horizontal CNC lathe 1 along the main axis direction, and mainly includes a longitudinal guide rail 6 and a transverse guide rail 7, the slide is arranged above the guide rail assembly 5, the tool holder is installed on one side of the slide, and the laser support frame 16 is installed on the other side of the slide; the ultrasonic rolling assembly is installed on the tool holder, and the ultrasonic rolling head 22 and the laser assembly 13 are synchronously moved horizontally along the x and z axes through the longitudinal and transversely arranged guide rails of the guide rail assembly 5. The three-jaw chuck 2 and the ejector 3 are coaxially arranged to fix the two ends of the workpiece respectively, and the bottom of the ejector 3 is installed on the transverse guide rail 7 of the guide rail assembly 5.
[0071] During processing, first, one end of the workpiece 34 to be strengthened is clamped on the horizontal CNC lathe 1 with the help of the three-jaw chuck 2, which can drive the workpiece to rotate axially, and the other end is fixed with the ejector pin 3. The ultrasonic rolling component 20 and the laser component 13 are respectively fixed on the tool holder 8 and the laser support frame 16 of the horizontal CNC lathe 1, and the two can move synchronously horizontally along the x and z axes. The ultrasonic rolling head 22 is aligned with the outer circumference of the workpiece in line contact, and the laser focusing head 15 of the laser component 13 emits a laser focusing beam that irradiates the contact area between the ultrasonic rolling component and the workpiece, and the position of the laser focusing head 15 and the laser incident angle θ can be adjusted; the thermometer 31 is connected to the industrial computer to monitor the surface temperature of the workpiece to be strengthened in real time; the laser movement speed v l The rolling speed v of the ultrasonic rolling assembly 20 r same.
[0072] Figure 3 Schematic diagram of the structure of the ultrasonic rolling assembly 20, the ultrasonic rolling assembly mainly includes an ultrasonic generator, a transducer 26, a horn 25, a fixing ring 28 and an ultrasonic rolling tool 21. The ultrasonic generator is placed in an integrated ultrasonic rolling device 30 and connected to one end of the transducer 26 inside the ultrasonic rolling assembly 20. The internal connection sequence is as follows: the other end of the transducer 26 is connected to the large end of the horn 25. At the same time, the small end of the horn is connected to the ultrasonic rolling head 22 by a positioning screw II 23. In addition, the fixing ring 28 is connected to the ultrasonic rolling fixture 29 by a bolt 27. Specifically, the axes of the transducer 26, the amplitude transformer 25, the ultrasonic rolling head 22, the fixing ring 28 and the ultrasonic rolling fixture 29 are located on the same straight line. The high-frequency AC signal generated by the ultrasonic generator is transmitted to the transducer 26, and the ultrasonic frequency electrical signal is converted into ultrasonic mechanical vibration by the transducer. After being amplified by the amplitude transformer 25, the mechanical vibration with a certain amplitude is output and transmitted to the ultrasonic rolling head 22, and acts on the outer peripheral surface of the workpiece 34 to be strengthened. The cross-section of the amplitude transformer is an isosceles trapezoid, and the transducer is a cylinder, and the diameters of the connecting ends of the two are the same.
[0073] Figure 4 The assembly sequence diagram of the tool holder 8 and the ultrasonic rolling assembly 20 is shown in FIG. Figure 3 The ultrasonic rolling fixture 29 of the ultrasonic rolling assembly 20 is provided with side wings on the side, and the ultrasonic rolling assembly 20 is clamped on the tool holder 8 by means of the side wings, through the fixer 9 and the positioning screw 10, and adjusted and fixed by the clamping nut 11 and the positioning screw Ⅰ12, and then the ultrasonic rolling head 22 is horizontally moved along the x and z axes through the slide 4, the longitudinal guide rail 6 and the transverse guide rail 7.
[0074] Figure 51 is a schematic diagram of the structure of the laser assembly 13. The laser assembly 13 mainly includes a laser controller 14, a laser focusing head 15 and a support frame 16 for fixing the laser assembly. A 360° rotation adjustment device 17 is provided between the laser focusing head 15 and the laser support frame 16 to adjust the horizontal rotation of the laser focusing head 15. The laser controller is connected to the laser focusing head 15 via an optical fiber. The support frame 16 includes a vertical support and a horizontal frame body. The overall shape is "cross-shaped". A lifting adjustment device 18 is provided on the top of the laser support frame, and the bottom is fixed on the other side of the slide 4 of the horizontal CNC lathe 1. Specifically, the position of the horizontal frame body on the vertical support is adjusted by the lifting adjustment device 18 on the support frame 16, thereby driving the laser focusing head 15 to move up and down along the y-axis. The laser focusing head 15 is fixed on the slide 4 of the horizontal CNC lathe 1 along the longitudinal and transverse guide rails in the guide rail assembly 5 to achieve horizontal movement along the x and z axes.
[0075] In this embodiment, the temperature measuring instrument 31 and the laser assembly 13 are both connected to the industrial computer, and the industrial computer includes a computer 32 and a host computer 33 .
[0076] In this embodiment, the ultrasonic rolling head 22 is a detachable elliptical ball with a hardness of HRC 60-92; a cooling lubrication hole 24 is provided on the ultrasonic rolling head 22, and the cooling lubrication hole 24 is connected to the integrated ultrasonic rolling device through a cooling hose laid on the outside of the ultrasonic rolling assembly 20, and is cooled by air.
[0077] In particular, while ultrasonic rolling strengthening is being performed, applying a temperature field (assisted by laser thermal softening) can achieve thermal softening of the workpiece material, further improving the mechanical properties of the material. Compared with a single ultrasonic rolling strengthening process, it can induce a deeper plastic deformation layer, further inhibiting cracking, shedding or cracking on the surface of the strengthened workpiece, as further illustrated in the following embodiments.
[0078] Embodiment 2
[0079] The present invention also provides a process for a laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device, which specifically includes the following steps:
[0080] Step 1: One end of the workpiece material 34 to be strengthened is horizontally clamped on the three-jaw chuck 2 of the horizontal CNC lathe 1, and the other end is fixed with the ejector 3; the ultrasonic rolling assembly 20 and the laser assembly 13 are respectively fixed on the tool holder 8 and the laser support frame 16, and the tool holder 8 and the laser support frame 16 are respectively arranged on both sides of the slide 4. Through the cooperation of the laser 360° rotation adjustment device 17, the lifting adjustment device 18 and the horizontal adjustment device composed of the guide rail assembly 5, the ultrasonic rolling head 22 is contacted and aligned with the outer circumference of the workpiece in a line contact manner, and the laser focusing head 15 irradiates the laser focusing beam to the contact area between the ultrasonic rolling and the workpiece to be strengthened.
[0081] In order to make the temperature distribution of the ultrasonic rolling area as uniform as possible, preferably, an elliptical spot 19 is selected. Specifically, the position of the laser focusing head 15 and the laser incident angle θ are adjusted by a 360° rotating adjustment device 17 and a lifting adjustment device 18 on the support frame 16 to change the position.
[0082] Step 2: Turn on the laser controller 14 and irradiate the generated laser beam to the outer edge of the workpiece to be strengthened through the laser focusing head 15 to thermally soften the surface of the workpiece to be strengthened. At the same time, the industrial computer monitors the temperature T of the surface of the workpiece to be strengthened in real time through the temperature meter 31.
[0083] Step 3: Adjust the laser parameters according to the monitored temperature T. When the temperature T is greater than the preset laser thermal softening auxiliary temperature threshold T1, that is, T>T1, where the preset laser thermal softening auxiliary temperature threshold T1 is the melting point of the workpiece material, adjust the laser parameters and laser position through the laser, and change the focused laser beam spot into an elliptical spot. Under the premise of ensuring that the workpiece material is not burned, the thermal softening effect of the laser helps to change the mechanical properties of the workpiece material, so that the plastic deformation resistance of the surface layer of the strengthening zone is appropriately reduced.
[0084] In this embodiment, the workpiece material 34 to be strengthened is a high temperature alloy GH4169, and the preset laser thermal softening auxiliary temperature threshold T1 is in the range of 650°C to 700°C; the laser parameters are as follows: the selection range of the spot diameter D is 50 to 80 μm, the selection range of the laser power P is 6 to 9 W, and the laser moving speed v l The selection range is 40-80 m / min, and the circumferential distance L between the center of the light spot and the center of the ultrasonic rolling tool is controlled in the range of 0.5-2 mm.
[0085] Step 4: At the same time, start the spindle, so that the three-jaw chuck 2 drives the workpiece to rotate, and set the ultrasonic rolling parameters through the machine tool program, and realize the joint adjustment and control of the laser component 13 and the ultrasonic rolling component 20 at the same position, thereby achieving the purpose of multi-energy field synchronous coupling and strengthening treatment of the workpiece. The entire operation process is realized on the horizontal CNC lathe 1.
[0086] The laser moving speed v l Should be related to the rolling speed v r Same. Combined Figure 6 , rolling depth a p and feed rate v f The following conditions should be met:
[0087] v l =v r =πDn (8)
[0088] a p =2bsinθ (9)
[0089] v f =a p tanθ=2bsinθtanθ (10)
[0090] Where: D is the workpiece diameter, n is the spindle speed.
[0091] Step 5: After the processing is completed, turn off the laser controller 14, turn off the horizontal CNC lathe 1 and the integrated ultrasonic rolling device 30, take out the workpiece, and monitor the temperature effect of the rolling area in real time using the test site and infrared thermometer. Figure 7 As shown, it can be seen that through this monitoring, the temperature change in the rolling area can be predicted more accurately, thereby realizing real-time adjustment of ultrasonic rolling and laser process parameters, ensuring that the temperature during the processing is always controlled at the preset threshold value T1 near the melting point of the workpiece material, preventing the material from overheating and melting and burning, and ensuring the processing quality and efficiency.
[0092] In step 3 and step 4: the laser process parameters and the ultrasonic rolling parameter range are optimized and selected based on finite element simulation and laser moving speed matching thermal softening test. The flow chart is as follows: Figure 8 As shown, the specific steps are as follows:
[0093] Step 1: Based on the heat transfer and mechanical properties of the material, combined with the empirical formula of laser thermal softening temperature, the finite element analytical numerical model of laser thermal softening temperature field distribution is established using MATLAB software to obtain the influence of different laser process parameters on the temperature and thermal stress of the workpiece surface, and then narrow the range of laser process parameters to ensure that the workpiece material surface does not have surface defects such as overburning and melting, and the thermal stress is too large to cause micro cracks on the workpiece surface. The finite element simulation is as follows: Fig. 9 As shown;
[0094] Step 2: Compare the workpiece surface temperature T under different laser process parameters with the preset laser thermal softening auxiliary temperature threshold T1, and preliminarily select the laser process parameter range in combination with the selection principle of ultrasonic rolling parameters;
[0095] Step 3: Verify and optimize the preliminary laser process parameters and ultrasonic rolling parameter range through laser moving speed matching thermal softening process test. The ultrasonic rolling process parameters are as follows: ultrasonic frequency f is 15-28kHz, ultrasonic amplitude A is 5-20μm, rolling depth a is 100-1500μm, and ultrasonic rolling depth f is 100-1500μm. p The workpiece spindle speed n is 300~650m / min.
[0096] Embodiment 3
[0097] The laser thermal softening assisted ultrasonic rolling synchronous strengthening device of the present invention is used and a group is selected from the preferred process parameter range to perform surface strengthening on the GH4169 high-temperature alloy material. The selected parameters are: laser spot diameter 50μm, laser power 8.4W, laser moving speed 60m / min, the circumferential distance between the center of the laser spot and the center of the ultrasonic rolling tool is controlled at 1.5mm, the ultrasonic frequency is 27kHz, the ultrasonic amplitude is 20μm, the workpiece spindle speed is 500m / min, the rolling depth is 0.3mm, and single ultrasonic rolling surface strengthening is performed. The strengthened workpiece material and ultrasonic rolling parameters are completely consistent with those of the present invention. After the strengthened GH4169 high-temperature alloy material is ground and polished, a scanning electron microscope is used to observe the surface morphology and sub-surface morphology after strengthening, such as Fig.10 As shown by Fig.10 It can be seen that after strengthening by a single ultrasonic rolling strengthening technology, the surface is relatively smooth and evenly distributed, with a few surface defects such as grooves, microcracks, and adhesion, which will inevitably become the driving force for inducing fatigue crack initiation. Compared with the single ultrasonic rolling strengthening technology, after the laser thermal softening assisted ultrasonic rolling synchronous strengthening device of the present invention and the preferred composite process parameters are used for strengthening treatment, the surface obtains a better and more uniform surface morphology, and the surface defects are relatively reduced a lot, inducing a deeper plastic deformation layer, the thickness of which can reach 45μm. It is proved that the composite synchronous strengthening device of the present invention can effectively improve the strengthening effect, surface quality and mechanical properties of the GH4169 high temperature alloy.
[0098] In order to better reveal the true state of the synchronous strengthening effect of laser thermal softening assisted ultrasonic rolling by the present invention, the three-dimensional surface morphology and cross-sectional profile curves of the single ultrasonic rolling strengthening sample and the laser thermal softening assisted ultrasonic rolling strengthening sample were observed and compared by a three-dimensional laser confocal microscope. Fig.11As shown. It can be seen that the surface profile curve of the single ultrasonic rolling strengthening specimen is in the range of [-393,1115]nm. Relatively speaking, after laser-assisted ultrasonic rolling, the two-dimensional surface profile curve becomes relatively smooth, and its surface profile curve is in the range of [-383,846]nm, which significantly reduces the surface roughness of the material, thereby greatly reducing the surface ups and downs, and the stress concentration effect will also be reduced, which has a good inhibitory effect on the initiation of microcracks and greatly improves the fatigue performance of the specimen.
[0099] Although the specific embodiments of the present invention are described above, it should be pointed out that a person skilled in the art may make several changes and improvements without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device, characterized in that: The invention comprises a horizontal CNC lathe, an ultrasonic rolling assembly, a laser assembly, a temperature measuring instrument and an industrial computer; one end of a workpiece (34) to be strengthened is clamped on the horizontal CNC lathe (1) and can drive the workpiece to rotate axially, and the other end is fixed by a pin (3); a guide rail assembly (5) is arranged on the processing side of the horizontal CNC lathe (1) along the main axis direction, an ultrasonic rolling assembly (20) and a laser assembly (13) are fixed above the guide rail assembly (5), and the two can move synchronously horizontally along the x and z axes; an ultrasonic rolling head (20) of the ultrasonic rolling assembly (20) 2) The laser focusing head (15) of the laser assembly (13) is in contact with and aligned with the outer circumference of the workpiece material to be strengthened, and the laser focusing beam emitted by the laser focusing head (15) of the laser assembly (13) is irradiated on the contact area between the ultrasonic rolling assembly and the workpiece material to be strengthened, and the position of the laser focusing head (15) and the laser incident angle θ can be adjusted; the temperature measuring instrument (31) is connected to an industrial computer to monitor the surface temperature of the workpiece to be strengthened in real time; the industrial computer includes a computer (32) and a computer host (33); the strengthened workpiece (34) is a high-strength, low-plasticity, difficult-to-process high-temperature alloy material.
2. The laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 1 is characterized in that: The horizontal CNC lathe comprises a guide rail assembly, a three-jaw chuck, an ejector pin, a slide, and a tool holder; the guide rail assembly comprises a longitudinal guide rail and a transverse guide rail, the transverse guide rail being arranged along the main axis of the horizontal CNC lathe, and the longitudinal guide rail being vertically movably mounted on the transverse guide rail; the slide plate (4) is arranged above the guide rail assembly (5), and the tool holder (8) and the laser support frame (16) are respectively mounted on both sides of the slide plate (4); the ultrasonic rolling assembly (20) is mounted on the tool holder (8), and the laser assembly (13) is mounted on the laser support frame (16); the ultrasonic rolling head (22) and the laser assembly (13) are synchronously moved horizontally along the x and z axes by the longitudinally and transversely arranged guide rails of the guide rail assembly (5); the three-jaw chuck (2) and the ejector pin (3) are coaxially arranged to fix the two ends of a workpiece respectively, and the bottom of the ejector pin (3) is mounted on the transverse guide rail (7) of the guide rail assembly (5).
3. The laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 1 is characterized in that: The ultrasonic rolling assembly mainly comprises an ultrasonic generator, a transducer, an amplitude change rod, a fixing ring, and an ultrasonic rolling tool. The ultrasonic rolling tool (21) adopts a rolling head in the form of a ball. The ultrasonic generator is placed in an integrated ultrasonic rolling device and connected to one end of the transducer inside the ultrasonic rolling assembly. The other end of the transducer is connected to the large end of the amplitude change rod. The small end of the amplitude change rod and the ultrasonic rolling head are connected by a positioning screw. The ultrasonic frequency electrical signal is converted into an ultrasonic mechanical vibration by the transducer (26). After being amplified by the amplitude change rod (25), the mechanical vibration with a certain amplitude is output and transmitted to the ultrasonic rolling tool (21), and acts on the workpiece to be strengthened. The cross section of the amplitude change rod is an isosceles trapezoid, and the transducer (26) is a cylinder. The diameters of the connecting ends of the two are the same.
4. The laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 3 is characterized in that: The ultrasonic rolling head has a detachable elliptical ball with a hardness of HRC 60-92; a cooling lubrication hole is provided on the ultrasonic rolling head, and the cooling lubrication hole is connected to the integrated ultrasonic rolling device through a cooling hose laid on the outside of the ultrasonic rolling assembly, and is cooled by air.
5. The laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 1, characterized in that: The laser assembly comprises a laser controller, a laser focusing head and a support frame for fixing the laser assembly. The laser is connected to the laser focusing head via an optical fiber. The support frame (16) comprises a vertical support and a horizontal frame body. The overall shape is a "cross shape". The bottom is arranged on the slide and fixed on the transverse guide rail. A 360° rotation adjustment device is arranged between the laser focusing head and the support frame, and the laser incident angle is adjusted by the 360° rotation adjustment device, thereby adjusting the diameter and shape of the light spot incident on the workpiece surface. A lifting adjustment device is arranged on the support frame. The support frame is lifted and lowered along the y-axis by the lifting adjustment device. The slide realizes the horizontal movement of the laser focusing head along the x-axis and the z-axis through the longitudinal and transverse guide rails of the guide rail assembly.
6. The operating process of the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 1 is characterized in that: The specific steps are as follows: Step 1: Clamp the workpiece to be strengthened on the three-jaw chuck of the horizontal CNC lathe and fix it with a thimble; fix the ultrasonic rolling assembly and the laser assembly on the tool holder and the laser support frame on both sides of the slide respectively, adjust the steering of the laser focusing head through the laser 360° rotation adjustment device, adjust the y-axis lifting movement of the laser focusing head through the lifting adjustment device, and adjust the horizontal movement of the x-axis and z-axis through the horizontal adjustment device composed of the slide and guide rail assembly, so that the ultrasonic rolling head and the outer peripheral surface of the workpiece to be strengthened are contacted and aligned in a line contact manner, and the laser focusing beam emitted by the laser focusing head irradiates the contact area between the ultrasonic rolling and the workpiece to be strengthened; Step 2: Turn on the laser controller and irradiate the generated laser beam through the laser focusing head to the contact area between the ultrasonic rolling component and the workpiece to be strengthened, so as to thermally soften the surface of the workpiece to be strengthened. At the same time, the industrial computer monitors the temperature T of the surface of the workpiece to be strengthened in real time through the temperature measuring instrument; Step 3: adjusting the laser parameters according to the monitored temperature T. When the temperature T is greater than the preset laser thermal softening auxiliary temperature threshold T1, that is, T>T1, where the preset laser thermal softening auxiliary temperature threshold T1 is the melting point of the workpiece material, the laser parameters are adjusted by the laser. Under the premise of ensuring that the workpiece material is not burned, the mechanical properties of the workpiece material are changed by means of the thermal softening effect of the laser, so that the plastic deformation resistance of the surface layer of the strengthening zone is appropriately reduced, so as to achieve the purpose of laser thermal softening assisted ultrasonic rolling; Step 4: At the same time, start the horizontal CNC lathe, make the three-jaw chuck drive the workpiece to rotate, set the ultrasonic rolling parameters and laser parameters, and realize the joint adjustment and control of the strengthening state of the laser component and the ultrasonic rolling component at the same position to realize the multi-energy field synchronous coupling strengthening treatment of the workpiece; The laser moving speed v l Should be related to the rolling speed v r Same; rolling depth a p and feed rate v f The following conditions should be met: v l =v r =πDn(8) a p =2bsinθ (9) v f =a p tanθ=2bsinθtanθ (10) Where: D is the workpiece diameter, n is the spindle speed; Step 5: After the processing is completed, turn off the laser controller (14), the horizontal CNC lathe (1) and the integrated ultrasonic rolling device (30), and take out the workpiece.
7. The operating process of the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 6 is characterized in that: In step 1, the laser emitted from the laser focusing head is controlled to irradiate the workpiece to be strengthened, and the circumferential distance between the center of the spot and the center of the ultrasonic rolling head is controlled within a range of 0.5 to 2 mm; In step 2, the workpiece material to be strengthened is the high temperature alloy GH4169, and the preset laser thermal softening auxiliary temperature threshold T1 is in the range of 650°C to 700°C; In step 3, the laser parameters submitted are as follows: spot diameter D is 50-80 μm, laser spot shape is elliptical, laser power P is 6-9 W, laser moving speed v l The ultrasonic rolling process parameters are as follows: ultrasonic frequency f is 15 to 28 kHz, ultrasonic amplitude A is 5 to 20 μm, rolling depth a p The workpiece spindle speed n is 300-650m / min; In step 4, when performing composite synchronous rolling strengthening, the axis of the ultrasonic rolling head should be perpendicular to the axis of the workpiece material to be strengthened, parallel to the center line of the laser spot along the circumferential direction of the workpiece to be strengthened, and the ultrasonic rolling head should be aligned with the workpiece.
8. The operating process of the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 6 is characterized in that: In step 1, the circumferential distance L between the center of the laser spot and the center of the ultrasonic rolling head can be calculated based on the angle β between the center of the ultrasonic rolling head and the center of the light beam in the cross section of the workpiece, the laser incident angle θ, and the radius R of the workpiece, and the relationship is:
9. The operating process of the laser thermal softening assisted ultrasonic rolling composite synchronous strengthening device according to claim 6 is characterized in that: The laser parameters and the ultrasonic rolling parameter range are optimized and selected based on finite element simulation and laser moving speed matching thermal softening test, and the specific steps are as follows: Step 1: Based on the heat transfer and mechanical properties of the material and the empirical formula of laser thermal softening temperature, a finite element analytical numerical model of laser thermal softening temperature field distribution is established using MATLAB software to obtain the influence of different laser process parameters on the temperature and thermal stress of the workpiece surface; Step 2: Compare the workpiece surface temperature T under different laser process parameters with the preset laser thermal softening auxiliary temperature threshold T1, and preliminarily select the laser process parameter range in combination with the selection principle of ultrasonic rolling parameters; When the laser spot shape is elliptical and the laser incident angle is θ, the major semi-axis a and minor semi-axis b of the elliptical spot are: a=r b secθ (1) b=r b (2) At this time, the laser power density distribution of the laser irradiating the workpiece surface should satisfy: Where: E is the laser beam power density at different positions on the cross section, W / m 2 ; P is laser power, W; r b is the spot radius of the laser effective area, mm; L is the circumferential distance from different positions of the cross section (rolling point) to the center of the laser spot, mm; Empirical formula for the temperature T in the laser processing area of cylindrical bars: Where λ is the thermal conductivity of the material, K is the diffusion coefficient, and t is the laser processing time. The temperature T of the laser processing area can be obtained by equations (3) and (4): Step 3: Verify through laser moving speed matching thermal softening process test, and optimize the preliminary laser process parameters and ultrasonic rolling process parameter range.
Citation Information
Cited By
Ultralow-plasticity, high-strength and high-hardness medium and low temperature forming technology
CN120133522A
A method for forming a high-strength high-hardness silicon carbide aluminum alloy at low temperature
CN120133522B
Laser compounding-rolling annealing method for high-strength stainless steel composite plate
CN120243637A
Twisting shaping machine
CN120551243A
Ultrahigh-strength steel rolling forming method and system, electronic equipment and storage medium
CN121339246A