Antifouling super-smooth hydrophobic coating as well as preparation method and application thereof
Through low-pressure continuous stirring technology, the sol matrix is uniformly mixed with the micro-nano additives to form an anti-fouling ultra-slip hydrophobic coating with excellent hydrophobicity and wear resistance, which solves the problem of poor mechanical stability of the micro-nano structure and achieves high resistance to the coating Abrasive and anti-fouling properties, suitable for a variety of applications.
Patent Information
- Application Number
- CN202411217824.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The poor mechanical stability of the existing micro-nano structures leads to the loss of super-hydrophobic and anti-fouling properties, making it difficult to maintain anti-fouling and waterproofing effects on the surface of the material for a long time.
The sol matrix and micro-nano additives are uniformly mixed with low pressure continuous stirring technology to form an anti-fouling ultraslip hydrophobic coating with excellent hydrophobicity and wear resistance. The nucleation and growth of condensate and ice are suppressed through the microsphere + nanowire structure. Improves the mechanical properties and bonding power of the coating.
It achieves high wear resistance, anti-fouling, anti-ice and anti-condensation properties of the coating, extends the service life of the material surface, reduces maintenance costs, and is suitable for industrial, aviation, aerospace and other fields.
Smart Images

Figure CN119060632A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material surfaces, and in particular relates to an antifouling super-slip hydrophobic coating and a preparation method and application thereof. Background Art
[0002] Wear resistance, waterproofness and antifouling are among the most important properties of material surfaces. For example, if dust and dirt adhere to the surfaces of mechanical parts, oil pipelines, kitchen utensils, walls and other materials such as aerospace vehicles, hulls, medical equipment, motor vehicles, wind turbine blades, it will cause further damage and corrosion to the subsequent material surface, thus causing great harm. Antifouling hydrophobic coatings can greatly reduce the adhesion of water, oil and pollutants on the surface to be protected, thereby effectively reducing the adhesion, long-term infiltration and accumulation of water molecules and pollutants. With the in-depth study of the superhydrophobic properties of the lotus leaf surface, researchers have found that the presence of micro-nano structures can reduce the adhesion between water, pollutants and organisms and the surface to be protected, and play a waterproof and antifouling role. However, the current application challenge of this technology lies in the poor mechanical stability of the micro-nano structure. External forces will cause certain damage to the micro-nano structure, and damage to the micro-nano structure will lead to the loss of superhydrophobic and antifouling properties. Summary of the invention
[0003] In view of this, the object of the present invention is to provide an anti-fouling super-slippery hydrophobic coating and a preparation method and application thereof. The coating formed by the anti-fouling super-slippery hydrophobic coating has excellent hydrophobicity and wear resistance and has good bonding with the substrate.
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] The present invention provides an antifouling super-slip hydrophobic coating, wherein the raw materials for preparing the coating include the following components in parts by mass:
[0006]
[0007] Preferably, the sol matrix includes one or more of silane, silicone rubber, silicone resin and epoxy resin.
[0008] Preferably, the silane includes one or more of trichlorosilane, trimethylsilane, trivinylsilane, triethoxysilane, tetraethoxysilane, silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent KH792, γ-(methacryloyloxy)propyltrimethoxysilane, silane coupling agent DL602 and silane coupling agent DL171.
[0009] Preferably, the low surface energy compound includes one or more of heptadecafluorodecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, stearic acid and polydimethylsiloxane.
[0010] Preferably, the micro-nano additive includes one or more of TiO2, SiO2, ZnO, Al2O3, Fe3O4, Fe2O3, paraffin, candle ash, polymethyl methacrylate, polyethylene, poly-isoprene siloxane and graphene.
[0011] Preferably, the particle size of the micro-nano additive is 10 nm to 20 μm.
[0012] The present invention also provides a method for preparing the antifouling super-slip hydrophobic coating described in the above technical solution, comprising the following steps:
[0013] The sol matrix, part of the low surface energy compound, water and part of the organic solvent are first mixed, and first stirred under a first low pressure environment to obtain a sol matrix solution;
[0014] The micro-nano additive, the remaining low surface energy compound and the remaining organic solvent are mixed for the second time, and low-pressure ultrasonic dispersion is performed to obtain a dispersion of the micro-nano additive; the mass ratio of the part of the low surface energy compound and the remaining low surface energy compound is (1-10):(0-5);
[0015] The sol matrix solution and the dispersion of the micro-nano additive are mixed for a third time, and stirred for a second time under a second low-pressure environment to obtain the antifouling super-slippery hydrophobic coating.
[0016] Preferably, the pressures of the first low-pressure environment and the second low-pressure environment are both 0.05 MPa.
[0017] The present invention also provides the use of the anti-fouling super-slippery hydrophobic coating described in the above technical scheme or the anti-fouling super-slippery hydrophobic coating prepared by the preparation method described in the above technical scheme in anti-icing, anti-condensation water or anti-fouling.
[0018] The present invention also provides a method for preparing an antifouling super-slippery hydrophobic coating, comprising the following steps:
[0019] The antifouling super-slippery hydrophobic coating is applied on the surface of the substrate and dried to obtain an antifouling super-slippery hydrophobic coating;
[0020] The antifouling super-slippery hydrophobic coating is the antifouling super-slippery hydrophobic coating described in the above technical solution or the antifouling super-slippery hydrophobic coating prepared by the preparation method described in the above technical solution.
[0021] The invention provides an antifouling super-slippery hydrophobic coating. The raw materials for preparing the coating include the following components, measured by weight: 10 parts of a sol matrix, 0.0001 to 10 parts of a low surface energy compound, 0 to 25 parts of a micro-nano additive, 5 to 400 parts of an organic solvent, and 0 to 10 parts of water.
[0022] The micro-nano additives in the coating formed by the antifouling super-slip hydrophobic coating provided by the present invention are uniformly dispersed in the sol (or gel) matrix, which not only effectively reduces the porosity or surface roughness of the coating caused by particle aggregation, but also significantly improves the mechanical properties of the coating, so that it has excellent wear resistance, and the coating material can also be closely combined with the substrate material, solve the problem of poor surface adhesion between the coating and the substrate material, and improve the contact area and bonding force between the coating and the substrate. Low surface energy compounds uniformly modify micro-nano additives and sol matrix, resulting in surface tensions less than deionized water and droplets greater than or equal to ethanol, which can slide freely from the coating surface without residue, thereby achieving antifouling performance. In addition, due to the special micro-nano structure and surface properties of the micron ball + nanowire of the coating, the nucleation and growth of condensed water and ice can be effectively suppressed, and the adhesion of ice is effectively reduced, so that the coating has the advantages of antifouling, anti-icing and anti-condensed water.
[0023] The present invention also provides a method for preparing the above-mentioned antifouling super-slip hydrophobic coating. The present invention slows down the movement of liquid molecules by adopting low-pressure continuous stirring technology, and the micro-nano additives are evenly dispersed in the sol matrix, thereby obtaining a high visible light transmittance. In addition, the uniform dispersion of the micro-nano additives effectively reduces the porosity or surface roughness of the coating caused by particle aggregation, thereby significantly improving the mechanical properties of the coating. The preparation method of the present invention is simple, the operation process is stable, the investment cost is low, the economic benefit is high, and it is easy to realize industrial production, and can be applied to the surfaces of metals, non-metals, organics, inorganics and various composite materials of various sizes and shapes. The antifouling super-slip hydrophobic coating prepared by the present invention is expected to replace the coating that pollutes and harms the water environment, and is suitable for operating environments such as drag reduction, corrosion prevention, anti-fouling, anti-icing, and anti-condensation water. It has a wide range of applications in the fields of industry, aviation, aerospace, navigation, outdoor buildings, and various engines, compressors, refrigerators, etc., and can extend the service life of the protected objects, reduce daily and special environmental consumption, save maintenance costs, and have good application value and economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a physical picture of the solution of the anti-fouling super-slippery hydrophobic coating prepared in Example 1;
[0025] Figure 2 This is a physical picture of the transparent antifouling super-slippery hydrophobic coating prepared in Example 2;
[0026] Figure 3 This is a surface contact angle diagram of the transparent antifouling super-slippery hydrophobic coating prepared in Example 1;
[0027] Figure 4 This is a surface rolling angle diagram of the transparent antifouling super-slippery hydrophobic coating prepared in Example 1;
[0028] Figure 5 This is a SEM image of the surface morphology of the transparent antifouling super-slippery hydrophobic coating prepared in Example 1;
[0029] Figure 6 This is a cross-sectional SEM image of the surface of the transparent antifouling super-slippery hydrophobic coating prepared in Example 1;
[0030] Figure 7 TEM image of the distribution of filling particles in the anti-fouling super-slippery hydrophobic coating prepared in Example 1 of the present invention;
[0031] Figure 8 TEM image of the distribution of filling particles in the anti-fouling super-slippery hydrophobic coating prepared in Example 3 of the present invention;
[0032] Fig. 9 This is a result diagram of the visible light transmittance of the anti-fouling super-slippery hydrophobic coatings prepared in Examples 1 and 2 of the present invention applied on a glass slide;
[0033] Fig.10 This is a cross-knife cutting test result diagram of the anti-fouling super-slippery hydrophobic coating prepared in Example 1 of the present invention;
[0034] Fig.11 This is a diagram showing the antifouling test results of the antifouling super-slippery hydrophobic coating prepared in Example 1 of the present invention;
[0035] Fig.12 This is a SEM image of the surface morphology of the translucent antifouling super-slippery hydrophobic coating prepared in Example 2;
[0036] Fig.13 This is a surface contact angle diagram of the translucent antifouling super-slippery hydrophobic coating prepared in Example 3;
[0037] Fig.14 This is a SEM image of the surface morphology of the antifouling super-slippery hydrophobic coating prepared in Example 3;
[0038] Fig.15 This is a SEM image of the surface morphology of the anti-fouling super-slippery hydrophobic coating prepared in Example 4;
[0039] Fig.16 This is the SEM image of the surface morphology of the anti-fouling super-slippery hydrophobic coating prepared in Example 5. DETAILED DESCRIPTION
[0040] The present invention provides an antifouling super-slippery hydrophobic coating, wherein the raw materials for preparing the coating include the following components in parts by mass:
[0041]
[0042] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used in the preparation, and commercially available products known to those skilled in the art can be used.
[0043] The preparation raw materials of the antifouling super-slippery hydrophobic coating provided by the present invention include a sol matrix having a mass fraction of 10. In the present invention, the sol matrix preferably includes one or more of silane, silicone rubber, silicone resin and epoxy resin, more preferably silane; the silane preferably includes trichlorosilane, trimethylsilane, trivinylsilane, triethoxysilane, tetraethoxysilane, silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent KH792, γ-(methacryloyloxy)propyltrimethoxysilane, silane coupling agent DL602 and silane coupling agent DL171, one or more of the above, more preferably trimethylsilane and silane coupling agent KH560; the mass ratio of the trimethylsilane and silane coupling agent KH560 is preferably 1:5; the trimethylsilane preferably includes methyltrimethoxysilane.
[0044] In the present invention, the silicone rubber includes dimethyl silicone rubber and / or methyl vinyl silicone rubber, more preferably methyl vinyl silicone rubber; the methyl vinyl silicone rubber is preferably a two-component methyl vinyl silicone rubber; the silicone resin preferably includes polydimethylsiloxane; the epoxy resin is preferably a two-component commercial epoxy resin. When the sol matrix is the above-mentioned types, the present invention has no special restrictions on the ratio of different types of sol matrices, and any ratio can be used.
[0045] Based on 1 mass fraction of the sol matrix, the raw materials for preparing the antifouling super-slippery hydrophobic coating provided by the present invention include 0.0001 to 10 mass fractions of low surface energy compounds, preferably 0.01 to 5 mass fractions. In the present invention, the low surface energy compound preferably includes one or more of heptadecafluorodecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, stearic acid and polydimethylsiloxane, more preferably heptadecafluorodecyltriethoxysilane. When the low surface energy compound is the above-mentioned several types, the present invention has no special restrictions on the ratio of different types of low surface energy compounds, and any ratio can be used.
[0046] In the present invention, the low surface energy compound is preferably used in the form of a low surface energy compound solution; the mass concentration of the low surface energy compound solution is preferably 0.1-20%, more preferably 1-10%; the solvent used for the low surface energy compound solution is preferably anhydrous ethanol or butyl acetate; the low surface energy compound solution is preferably a purchased product.
[0047] In the present invention, the low surface energy compound uniformly modifies the micro-nano additive and the sol matrix, resulting in that the droplets with surface tension less than deionized water and greater than or equal to ethanol can slide freely from the coating surface without residue, thereby achieving anti-fouling performance. In addition, due to the special structure and surface properties of the coating, the nucleation and growth of condensed water and ice can be effectively inhibited, and the adhesion of ice can be effectively reduced, thereby making the coating have the advantages of anti-fouling, anti-icing, and anti-condensation water.
[0048] Based on 1 mass fraction of the sol matrix, the raw materials for preparing the antifouling super-slip hydrophobic coating provided by the present invention include 0 to 25 mass fractions of micro-nano additives, preferably 0.5 to 10 mass fractions. In the present invention, the micro-nano additives preferably include one or more of TiO2, SiO2, ZnO, Al2O3, Fe3O4, Fe2O3, paraffin, candle ash, polymethyl methacrylate, polyethylene, poly-isoprene siloxane and graphene, more preferably TiO2, SiO2, paraffin, candle ash, poly-isoprene siloxane or graphene; the TiO2 preferably includes one or more of TiO2 particles, TiO2 fibers and TiO2 nanotubes, more preferably TiO2 particles; the particle size of the micro-nano additive is preferably 10nm to 20μm, more preferably 20nm to 200nm. When the micro-nano additives are the above-mentioned ones, the present invention does not specifically limit the ratio of different types of micro-nano additives, and any ratio is sufficient.
[0049] In the present invention, the micro-nano additive can be a mixture of the same kind of particles, fibers or nanotubes with different particle sizes, or a mixture of different kinds of compositions. In the embodiment of the present invention, the SiO2 is SiO2 nanoparticles; the TiO2 is TiO2 nanotubes; the ZnO is ZnO nanoparticles; the polymethyl methacrylate is polymethyl methacrylate microspheres; and the candle ash is candle ash particles.
[0050] In the present invention, the micro-nano additives are uniformly dispersed in the sol (or gel) matrix solution, which not only effectively reduces the porosity inside and on the surface of the coating caused by particle aggregation or the formation of a rough surface structure, thereby significantly improving the mechanical properties of the coating and making it have excellent wear resistance, but also allows the coating material to be tightly combined with the substrate material, thereby solving the problem of poor surface adhesion between the coating and the substrate material and increasing the contact area and bonding force between the coating and the substrate.
[0051] Based on 1 mass fraction of the sol matrix, the raw material for preparing the antifouling super-slippery hydrophobic coating provided by the present invention includes 5 to 400 mass fractions of organic solvent, preferably 20 to 200 mass fractions. In the present invention, the organic solvent preferably includes one or more of ethanol, methanol, tetrahydrofuran, diethyl oxalate, butyl acetate and xylene, more preferably ethanol or methanol. When the organic solvent is a mixture of the above two organic solvents, the volume ratio of the two organic solvents is preferably 1 to 5: 1 to 5, more preferably 1 to 3: 1 to 3.
[0052] Based on 1 mass part of the sol matrix, the raw materials for preparing the antifouling super-slippery hydrophobic coating provided by the present invention include 0 to 10 mass parts of water, preferably 1 to 8 mass parts, and more preferably 1 to 5 mass parts. In the present invention, the water is preferably deionized water.
[0053] The present invention also provides a method for preparing the antifouling super-slip hydrophobic coating described in the above technical solution, comprising the following steps:
[0054] The sol matrix, part of the low surface energy compound, water and part of the organic solvent are first mixed, and first stirred under a first low pressure environment to obtain a sol matrix solution;
[0055] The micro-nano additive, the remaining low surface energy compound and the remaining organic solvent are mixed for the second time, and low-pressure ultrasonic dispersion is performed to obtain a dispersion of the micro-nano additive; the mass ratio of the part of the low surface energy compound and the remaining low surface energy compound is (1-10):(0-5);
[0056] The sol matrix solution and the dispersion of the micro-nano additive are mixed for a third time, and stirred for a second time under a second low-pressure environment to obtain the antifouling super-slippery hydrophobic coating.
[0057] In the present invention, the pressure of the first low-pressure environment is preferably 0.05 MPa; the first stirring is preferably magnetic stirring; the rate of the first stirring is preferably 400-1000 rpm, more preferably 500-600 rpm; the time of the first stirring is preferably 2-48 h, more preferably 2-24 h; the temperature of the first stirring is preferably 0-30°C, more preferably 10-20°C.
[0058] In the present invention, the volume ratio of the part of the organic solvent to the remaining organic solvent is preferably 1-5:1-5, more preferably 2:1; the mass ratio of the part of the low surface energy compound to the remaining low surface energy compound is (1-10):(0-5), preferably (1-10):(0-1); the power of the low-pressure ultrasonic dispersion is preferably 20-40kHz, more preferably 30-40kHz; the time of the low-pressure ultrasonic dispersion is preferably 5-60min, more preferably 15-30min; the temperature of the low-pressure ultrasonic dispersion is preferably 0-30°C, more preferably 10-20°C; the pressure of the low-pressure ultrasonic dispersion is preferably 0.05MPa.
[0059] In the present invention, the pressure of the second low-pressure environment is preferably 0.05 MPa; the rate of the second stirring is preferably 500-800 rpm, more preferably 600 rpm; the time of the second stirring is preferably 2-600 h, more preferably 100-300 h; the stirring is preferably magnetic stirring; the temperature of the second stirring is preferably 0-30°C, more preferably 10-20°C.
[0060] The present invention uses low-pressure continuous stirring technology to slow down the movement of liquid molecules, and the micro-nano additives are evenly dispersed in the sol matrix, thereby obtaining a high visible light transmittance. In addition, the uniform dispersion of the micro-nano additives effectively reduces the porosity inside and on the surface of the coating or the formation of a rough surface structure caused by particle aggregation, thereby significantly improving the mechanical properties of the coating.
[0061] The present invention adopts low-pressure stirring technology to regulate the dispersion state of micro-nano powders, micro-nano particles, fibers and nanotubes in the sol, so as to obtain a stable super-slippery hydrophobic antifouling coating. The preparation method is simple, low-cost, and is generally applicable to the regulation of common powders and particles to prepare functional surfaces or super-slip surfaces of various micro-nano structures. The prepared super-slippery hydrophobic coating has a transmittance of 98%, a water drop contact angle greater than 100°, and a water rolling angle less than 50°. In addition, the coating formed by the coating has a good anti-fouling effect, and crude oil, edible oil and various solvents can slide down without residue. In addition, the coating formed by the coating has good wear resistance, anti-icing and anti-condensation water performance, and is expected to be used in anti-pollution, anti-icing and anti-condensation water coatings in the fields of industry, aviation and navigation.
[0062] The present invention also provides the use of the anti-fouling super-slippery hydrophobic coating described in the above technical scheme or the anti-fouling super-slippery hydrophobic coating prepared by the preparation method described in the above technical scheme in anti-icing, anti-condensation water or anti-fouling.
[0063] The present invention provides a method for preparing an antifouling super-slippery hydrophobic coating, comprising the following steps:
[0064] The antifouling super-slippery hydrophobic coating is applied on the surface of the substrate and dried to obtain an antifouling super-slippery hydrophobic coating;
[0065] The antifouling super-slippery hydrophobic coating is the antifouling super-slippery hydrophobic coating described in the above technical solution or the antifouling super-slippery hydrophobic coating prepared by the preparation method described in the above technical solution.
[0066] Before the coating, the present invention preferably cleans the surface of the substrate to remove surface impurities and contaminants. The present invention has no special limitation on the cleaning process, and any cleaning process known in the art can be used.
[0067] In the present invention, the coating is preferably spin coating, drip coating, brush coating, spray coating, leveling or scraper coating, more preferably spray coating; the drying temperature is preferably 30-150°C, more preferably 60-90°C; the drying time is preferably 0.2-24h, more preferably 1-6h.
[0068] The present invention preferably repeats the coating and drying process multiple times to adjust the thickness and refractive index of the antifouling super-slippery hydrophobic coating; the number of repetitions is preferably 1 to 4 times, more preferably 3 times.
[0069] In the present invention, the thickness of the antifouling super-slippery hydrophobic coating is preferably 10 to 30 μm, more preferably 15 to 25 μm.
[0070] The present invention has no special restrictions on the material of the substrate, nor is it limited to a single substrate, and is widely applicable to various regular or irregular metal, non-metal, organic, inorganic and various composite material surfaces. In an embodiment of the present invention, the substrate is made of glass fiber reinforced resin, a glass slide, an aluminum alloy sheet, a titanium alloy, a carbon fiber plate, a stainless steel sheet or an aluminum mesh.
[0071] The anti-fouling ultra-slippery hydrophobic coating provided by the present invention has no micro-nano structure but has good mechanical properties. Not only is it not easy for oil, solvents, ice, frost, etc. to adhere or form, but it also has high transparency. In addition, the coating has high strength, high hardness, good bonding with the substrate, and anti-wear properties.
[0072] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.
[0073] Example 1
[0074] 10 mL of methanol, 0.55 g of methyltrimethoxysilane, 4.72 g of silane coupling agent KH560 and 1.50 g of deionized water were added to a covered glass bottle, and then 0.1 mL of heptadecafluorodecyltriethoxysilane was mixed with 10 mL of anhydrous ethanol and added to the above solution, and then part of the air was evacuated and the bottle cap was tightly sealed, and the low-pressure solution (0.05 MPa) in the glass bottle was magnetically stirred at 20° C. and 600 rpm for 4 h to obtain a sol matrix solution;
[0075] 1.5 g of SiO2 nanoparticles (particle size of 200 nm) were added to 10 mL of methanol and placed in an ultrasonic bath at a temperature of 20°C and a pressure of 0.05 MPa for 30 min at a power of 30 kHz to eliminate particle aggregation and obtain a SiO2 nanoparticle dispersion;
[0076] The sol matrix solution and the SiO2 nanoparticle dispersion were mixed, and stirred for 240 h at 20°C and a magnetic stirring speed of 600 rpm under a 0.05 MPa environment to obtain an antifouling super-slip hydrophobic coating;
[0077] The antifouling super-slippery hydrophobic coating was spin-coated on a clean substrate to be protected (glass fiber reinforced resin) and cured in an oven at 90° C. for 1.5 h to obtain an antifouling super-slippery hydrophobic coating (with a thickness of 10 μm).
[0078] Example 2
[0079] 15 mL of anhydrous ethanol, 0.63 g of trichlorosilane, 8.50 g of silane coupling agent KH550 and 1.84 g of deionized water were added to a covered glass bottle, and then 0.1 g of stearic acid was added to the above solution. After that, part of the air was evacuated and the bottle cap was tightly sealed. The low-pressure solution (0.05 MPa) in the glass bottle was magnetically stirred at 20° C. and 500 rpm for 24 h to obtain a sol matrix solution;
[0080] 0.8 g of TiO2 nanotubes (particle size of 50 nm) were added to 10 mL of tetrahydrofuran and placed in an ultrasonic bath at a temperature of 20°C and a pressure of 0.05 MPa for 15 min at a power of 40 kHz to eliminate particle aggregation and obtain a TiO2 nanotube dispersion;
[0081] The sol matrix solution and the TiO2 nanotube dispersion were mixed, and stirred for 450 hours at 20°C and a magnetic stirring speed of 600 rpm under a 0.05 MPa environment to obtain an antifouling super-slippery hydrophobic coating;
[0082] The antifouling super-slippery hydrophobic coating was sprayed on a clean substrate to be protected (a glass slide) and cured in an oven at 110° C. for 1.5 h to obtain an antifouling super-slippery hydrophobic coating (with a thickness of 10 μm).
[0083] Example 3
[0084] 10 mL of anhydrous ethanol, 0.55 g of tetraethoxysilane, 4.72 g of silane coupling agent KH560 and 1.50 g of deionized water were added to a covered glass bottle, and then 0.1 mL of heptadecafluorodecyltriethoxysilane was mixed with 10 mL of anhydrous ethanol and added to the above solution, and then part of the air was evacuated and the bottle cap was tightly sealed, and the low-pressure solution (0.05 MPa) in the glass bottle was magnetically stirred at 20° C. and 1000 rpm for 2 h to obtain a sol matrix solution;
[0085] 0.2 g of TiO2 nanotubes (tube diameter of 50 nm) and 1.0 g of SiO2 nanoparticles (particle diameter of 200 nm) were added to 10 mL of methanol and placed in an ultrasonic bath at a temperature of 20°C and a pressure of 0.05 MPa for 20 min at a power of 40 kHz to eliminate particle aggregation and obtain a dispersion containing TiO2 and SiO2;
[0086] The sol matrix solution and the dispersion containing TiO2 and SiO2 are mixed, and stirred for 600 hours at 20°C and 600 rpm under a 0.05 MPa environment until the solution is transparent to obtain an antifouling super-slip hydrophobic coating;
[0087] The antifouling super-slippery hydrophobic coating was drop-coated on a clean substrate to be protected (aluminum alloy sheet) and cured in an oven at 90° C. for 1.5 h to obtain an antifouling super-slippery hydrophobic coating (with a thickness of 10 μm).
[0088] Example 4
[0089] 10 mL of anhydrous ethanol, 2.00 g of diethyl oxalate, 0.65 g of γ-(methacryloyloxy)propyltrimethoxysilane and 0.50 g of deionized water were added to a covered glass bottle, and then 0.1 mL of heptadecafluorodecyltriethoxysilane was mixed with 10 mL of anhydrous ethanol and added to the above solution, and then part of the air was evacuated and the bottle cap was tightly sealed, and the low-pressure solution (0.05 MPa) in the glass bottle was magnetically stirred at 20° C. and 400 rpm for 2 h to obtain a sol matrix solution;
[0090] 0.5 g SiO2 nanoparticles (particle size of 200 nm) and 1.0 g SiO2 nanoparticles (particle size of 10-20 nm) were added to 10 mL methanol and placed in an ultrasonic bath at a temperature of 20°C and a pressure of 0.05 MPa for 15 min at a power of 40 kHz to eliminate particle aggregation and obtain a SiO2 nanoparticle dispersion;
[0091] The sol matrix solution and the SiO2 nanoparticle dispersion were mixed, and stirred for 350 h at 20°C and a magnetic stirring speed of 600 rpm under a 0.05 MPa environment to obtain an antifouling super-slip hydrophobic coating;
[0092] The antifouling super-slippery hydrophobic coating was coated on a clean substrate to be protected (titanium alloy) with a scraper and cured in an oven at 60°C for 0.5h, then heated to 100°C and continued to cure for 1.0h to obtain an antifouling super-slippery hydrophobic coating (thickness of 10 μm).
[0093] Example 5
[0094] 10 mL of butyl acetate, 0.2 g of trichlorosilane, 0.9 g of KH792 and 0.50 g of deionized water were added to a covered glass bottle, and then 0.1 mL of heptadecafluorodecyltriethoxysilane was mixed with 10 mL of anhydrous ethanol and added to the above solution. After that, part of the air was evacuated and the bottle cap was tightly closed and sealed. The low-pressure solution (0.05 MPa) in the glass bottle was magnetically stirred at 20° C. and 900 rpm for 2 h to obtain a sol matrix solution;
[0095] 1.0 g ZnO nanoparticles (particle size of 50 nm) and 0.01 mL tridecafluorooctyltrimethoxysilane were added to 10 mL butyl acetate and placed in an ultrasonic bath at a temperature of 20°C and a pressure of 0.05 MPa for 15 min at a power of 30 kHz to eliminate particle aggregation and obtain a ZnO nanoparticle dispersion;
[0096] The sol matrix solution and the ZnO nanoparticle dispersion were mixed, and stirred for 500 h at 20° C. and a magnetic stirring speed of 600 rpm under an environment of 0.05 MPa to obtain an antifouling super-slippery hydrophobic coating;
[0097] The antifouling super-slippery hydrophobic coating was leveled on a clean substrate to be protected (a carbon fiber board) and cured in an oven at 60°C for 0.5h, then heated to 100°C and continued to cure for 1.0h to obtain an antifouling super-slippery hydrophobic coating (thickness of 25 μm).
[0098] Example 6
[0099] 10 mL of anhydrous ethanol, 0.55 g of tetraethoxysilane, 4.72 g of silane coupling agent KH560 and 1.50 g of deionized water were added to a covered glass bottle, and then 0.01 mL of tridecafluorooctyltrimethoxysilane was added to the above solution. After that, part of the air was evacuated and the bottle cap was tightly sealed. The low-pressure solution (0.05 MPa) in the glass bottle was magnetically stirred at 20° C. and 700 rpm for 2 h to obtain a sol matrix solution.
[0100] 0.5 g of polymethyl methacrylate microspheres (particle size of 20 μm) and 0.5 g of SiO2 nanoparticles (particle size of 200 nm) were added to 10 mL of methanol and placed in an ultrasonic bath at a temperature of 20°C and a pressure of 0.05 MPa for 20 min at a power of 40 kHz to eliminate particle aggregation, thereby obtaining a dispersion of polymethyl methacrylate microspheres and SiO2 nanoparticles;
[0101] The sol matrix solution, polymethyl methacrylate microspheres and SiO2 nanoparticle dispersion were mixed, and stirred for 600 h at 20° C. and 600 rpm magnetic stirring speed under 0.05 MPa environment to obtain an antifouling super-slip hydrophobic coating;
[0102] The antifouling super-slippery hydrophobic coating was brushed onto a clean substrate to be protected (a stainless steel sheet) and cured in an oven at 90° C. for 1.5 h to obtain an antifouling super-slippery hydrophobic coating (with a thickness of 20 μm).
[0103] Example 7
[0104] 10 mL of anhydrous ethanol, 0.55 g of trivinylsilane, 5.00 g of polydimethylsiloxane and 1.50 g of deionized water were added to a covered glass bottle, and then 0.1 mL of heptadecafluorodecyltriethoxysilane was mixed with 10 mL of anhydrous ethanol and added to the above solution, and then part of the air was evacuated and the bottle cap was tightly sealed, and the low-pressure solution (0.05 MPa) in the glass bottle was magnetically stirred at 20° C. and 500 rpm for 2 h to obtain a sol matrix solution;
[0105] 0.5 g of candle ash particles (particle size of 20-200 nm) were added to 10 mL of xylene and placed in an ultrasonic bath at a temperature of 20°C and a pressure of 0.05 MPa for 15 min at a power of 40 kHz to eliminate particle aggregation and obtain a candle ash particle dispersion;
[0106] The sol matrix solution and the candle ash particle dispersion are mixed, and stirred for 100 hours at 20° C. and a magnetic stirring speed of 600 rpm under a container pressure of 0.05 MPa to obtain an antifouling super-slippery hydrophobic coating;
[0107] The antifouling super-slippery hydrophobic coating was spin-coated on a clean substrate to be protected (aluminum mesh) and cured in an oven at 90° C. for 1.5 h to obtain an antifouling super-slippery hydrophobic coating (with a thickness of 10 μm).
[0108] Comparative Example 1
[0109] According to the prior art (A novel slippery surface with enhanced stability and corrosion resistance. Progress in Organic Coatings, Vol 142, 2020, 105563), a smooth liquid-infused porous surface (SLIPS) was prepared by simultaneously introducing silica sol and carbon nanotubes (CNT) by a simple spraying method and then infusing oil. During the molten PVDF process, solvent evaporation and silica sol shrinkage form abundant micropores and nanopores, which both act as reservoirs for holding oil. The effect of CNT on oil holding capacity and corrosion inhibition mechanism was then studied in detail. The interaction between SiO2 nanoparticles and CNTs gives the original hierarchical structure a richer morphology and an increased number of micropores. These two factors synergistically enhance the ability to lock oil, indicating that the performance of SLIPS is more stable.
[0110] In Comparative Example 1, PVDF and carbon nanotubes are used to prepare a hierarchical structure, silicone oil is introduced, and the oil is locked through the pores on the coating surface to achieve super-slippery, while Example 1 can also achieve super-slippery without silicone oil filling. On the other hand, in Comparative Example 1, carbon nanotubes are mainly used to form a certain surface roughness structure, and SiO2 nanoparticles are prepared on the surface of carbon nanotubes and PVDF and between the cross-linked pores of the two by adding precursors and preparing them through chemical synthesis under the catalytic action of ammonia water, while in Example 1, micro-nano rough structures are prepared by directly adding low-cost SiO2 nanoparticles, using a sol matrix to construct uniform pores and form a stable cross-linked structure with SiO2 nanoparticles; in addition, the preparation process of Example 1 is carried out under a low-pressure environment, which is more conducive to the formation of a rich porous structure and more stable performance.
[0111] Comparative Example 2
[0112] The difference from Example 1 is that the silane coupling agent KH560 is not added.
[0113] Comparative Example 3
[0114] The difference from Example 1 is that the low surface energy compound, heptadecafluorodecyltriethoxysilane solution, is not added.
[0115] Comparative Example 4
[0116] The difference from Example 1 is that no micro-nano additive, i.e. SiO2 nanoparticles, is added.
[0117] Performance Testing
[0118] Figure 1 This is a real picture of the solution of the antifouling super-slippery hydrophobic coating prepared in Example 1. Figure 1It can be seen that the solution is clear and there is no aggregation of large particles.
[0119] Figure 2 This is a photo of the transparent antifouling super-slippery hydrophobic coating prepared in Example 2. Figure 2 It can be seen that the coating protects the original color of the substrate very well, and water droplets appear in the shape of water beads on the surface of the coating, showing hydrophobic properties.
[0120] Figure 3 This is a surface contact angle diagram of the transparent antifouling super-slippery hydrophobic coating prepared in Example 1. Figure 3 It can be seen that the contact angle of the prepared coating surface is 110°.
[0121] Figure 4 This is a surface rolling angle diagram of the transparent antifouling super-slippery hydrophobic coating prepared in Example 1. Figure 4 It can be seen that the sliding angle of the prepared coating surface is 40°.
[0122] Figure 5 This is a SEM image of the surface morphology of the transparent anti-fouling super-slippery hydrophobic coating prepared in Example 1. Figure 6 This is a cross-sectional SEM image of the surface of the transparent antifouling super-slippery hydrophobic coating prepared in Example 1. Figure 5 and Figure 6 It can be seen that the coating surface is smooth without pores or micro-nano structures, and the coating is tightly bonded to the substrate without obvious defects or gaps that affect its bonding strength.
[0123] Figure 7 This is a TEM image of the distribution of filling particles in the anti-fouling super-slippery hydrophobic coating prepared in Example 1 of the present invention. Figure 8 This is a TEM image of the distribution of filling particles in the anti-fouling super-slippery hydrophobic coating prepared in Example 3 of the present invention. Figure 7 and Figure 8 It can be seen that the nanoparticles and nanotubes are uniformly dispersed inside the coating without agglomeration, thereby effectively reducing the porosity and transparency of the coating.
[0124] Fig. 9 The results of the visible light transmittance of the antifouling super-slippery hydrophobic coatings prepared in Examples 1 and 2 of the present invention applied on a glass slide are shown in FIG. Fig. 9 It can be seen that the coatings prepared in Example 1 and Example 2 have very high visible light transmittance. When the coatings are coated on the surface of a glass slide, the visible light transmittance is as high as more than 85%.
[0125] Fig.10This is a cross-knife test result diagram of the anti-fouling super-slip hydrophobic coating prepared in Example 1 of the present invention. According to the ASTM D3359 international standard test method, the scratch resistance of the coating reaches the highest level 5B, indicating that a good bonding force is formed between the coating and the substrate, and the coating shows a certain toughness.
[0126] Fig.11 This is a graph showing the antifouling test results of the antifouling super-slippery hydrophobic coating prepared in Example 1 of the present invention. Fig.11 It can be seen that the oil stain can slide off the coating surface within 10 seconds without any residue.
[0127] Fig.12 This is a SEM image of the surface morphology of the semi-transparent antifouling super-slippery hydrophobic coating prepared in Example 2. Fig.12 It can be seen that the coating surface has a certain micro-protrusion structure caused by the aggregation of nanotubes, but no hole structure.
[0128] Fig.13 This is a surface contact angle diagram of the semi-transparent antifouling super-slippery hydrophobic coating prepared in Example 3. Fig.13 It can be seen that the contact angle of the prepared coating surface is 130°.
[0129] Fig.14 The SEM image of the surface morphology of the antifouling super-slippery hydrophobic coating prepared in Example 3. Fig.14 It can be seen that the nanotube cluster structure and the nanoparticle structure coexist.
[0130] Fig.15 The following is a SEM image of the surface morphology of the antifouling super-slippery hydrophobic coating prepared in Example 4. Fig.15 It can be seen that SiO2 particles of different sizes are evenly distributed on the coating surface.
[0131] Fig.16 The SEM image of the surface morphology of the antifouling super-slippery hydrophobic coating prepared in Example 5. Fig.16 It can be seen that a uniform pore structure is formed on the coating surface, and 50nm ZnO particles are evenly dispersed on the coating surface without agglomeration, providing the required uniform micro-nano structure for the anti-fouling ultra-slip coating.
[0132] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An antifouling super-slip hydrophobic coating, characterized in that: The raw materials for preparation include the following components by weight:
2. The antifouling super-slip hydrophobic coating according to claim 1, characterized in that: The sol matrix includes one or more of silane, silicone rubber, silicone resin and epoxy resin.
3. The antifouling super-slip hydrophobic coating according to claim 2, characterized in that: The silane includes one or more of trichlorosilane, trimethylsilane, trivinylsilane, triethoxysilane, tetraethoxysilane, silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent KH792, γ-(methacryloyloxy)propyltrimethoxysilane, silane coupling agent DL602 and silane coupling agent DL171.
4. The antifouling super-slip hydrophobic coating according to claim 1, characterized in that: The low surface energy compound includes one or more of heptadecafluorodecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, stearic acid and polydimethylsiloxane.
5. The anticorrosive coating according to claim 1, characterized in that: The micro-nano additives include one or more of TiO2, SiO2, ZnO, Al2O3, Fe3O4, Fe2O3, paraffin, candle ash, polymethyl methacrylate, polyethylene, poly-isoprene siloxane and graphene.
6. The anticorrosive coating according to claim 5, characterized in that: The particle size of the micro-nano additive is 10nm-20μm.
7. The method for preparing the antifouling super-slip hydrophobic coating according to any one of claims 1 to 6, characterized in that: The following steps are involved: The sol matrix, part of the low surface energy compound, water and part of the organic solvent are first mixed, and first stirred under a first low pressure environment to obtain a sol matrix solution; The micro-nano additive, the remaining low surface energy compound and the remaining organic solvent are mixed for the second time, and low-pressure ultrasonic dispersion is performed to obtain a dispersion of the micro-nano additive; the mass ratio of the part of the low surface energy compound and the remaining low surface energy compound is (1-10):(0-5); The sol matrix solution and the dispersion of the micro-nano additive are mixed for a third time, and stirred for a second time under a second low-pressure environment to obtain the antifouling super-slippery hydrophobic coating.
8. The preparation method according to claim 7, characterized in that: The pressures of the first low-pressure environment and the second low-pressure environment are both 0.05 MPa.
9. Use of the antifouling super-slippery hydrophobic coating according to any one of claims 1 to 6 or the antifouling super-slippery hydrophobic coating prepared by the preparation method according to claim 7 or 8 in anti-icing, anti-condensation water or anti-fouling.
10. A method for preparing an antifouling super-slippery hydrophobic coating, characterized in that: The following steps are involved: The antifouling super-slippery hydrophobic coating is applied on the surface of the substrate and dried to obtain an antifouling super-slippery hydrophobic coating; The antifouling super-slippery hydrophobic coating is the antifouling super-slippery hydrophobic coating according to any one of claims 1 to 6 or the antifouling super-slippery hydrophobic coating prepared by the preparation method according to claim 7 or 8.
Citation Information
Cited By
Super wear-resistant antifouling paint and preparation method thereof
CN120158190A
Super wear-resistant antifouling coating and preparation method thereof
CN120158190B
High-temperature-resistant anti-adhesion super-hard transparent fluorine-free green organic silicon coating and preparation method thereof
CN120795789A
A high-temperature-resistant anti-adhesion superhard transparent fluorine-free green silicone coating and a preparation method thereof
CN120795789B
Coating composition, and preparation method therefor and use thereof
WO2026137760A1