Negative Poisson's ratio buffer material and preparation process thereof

Through the preparation of negative Poisson's buffer material, dopamine-modified porous wood powder is used to improve the compatibility of polyethylene and polytetrafluoroethylene, forming a two-dimensional concave hexagonal honeycomb structure, solving the deformation problem of refrigerator door panels and significantly improving the deformation of the refrigerator door panel. The elasticity and impact resistance of the buffer layer are achieved.

CN118909339APending Publication Date: 2024-11-08ANHUI HIGASKET PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149522.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The elasticity of the buffer layer material of the refrigerator door panel is poor, which leads to the inability to effectively absorb the expansion force during foaming, causing the door panel to deform.

Method used

Using negative Poisson's ratio buffer material, composed of PE foam, dopamine-modified porous wood powder, PTFE and zinc oxide, a two-dimensional concave hexagonal honeycomb structure is formed through the preparation process to improve the phase between polyethylene and polytetrafluoroethylene. Capacitance and creep performance show negative Poisson's ratio effect.

Benefits of technology

Improve the elasticity of the buffer layer, enhance the resistance to deformation of the refrigerator door panel, improve the compatibility and structural interlock between polyethylene and polytetrafluoroethylene through dopamine-modified porous wood powder, forming an elastic sponge structure, which significantly improves the Surface impact absorption and rebound performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003236890000071
    Figure BDA0005003236890000071
  • Figure BDA0005003236890000081
    Figure BDA0005003236890000081
Patent Text Reader

Abstract

The invention discloses a negative Poisson's ratio buffer material and a preparation process thereof, and belongs to the technical field of auxetic materials, the negative Poisson's ratio buffer material is composed of PE foam, and the negative Poisson's ratio buffer material comprises the following components by mass: 80-100 parts of PE, 5-10 parts of a foaming agent, 10-25 parts of dopamine modified porous wood flour, 8-12 parts of PTFE, and 2-4 parts of zinc oxide; and the Poisson ratio of the PE foam is-1 to 0. The compatibility between polyethylene and polytetrafluoroethylene is improved by preparing dopamine modified porous wood powder, and meanwhile, the dopamine modified porous wood powder is used as a structural template to enable the polyethylene and the polytetrafluoroethylene to be mutually embedded, so that a two-dimensional concave hexagonal honeycomb structure is formed, and a remarkable negative Poisson's ratio effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of traction materials, and in particular relates to a negative Poisson's ratio buffer material and a preparation process thereof. Background Art

[0002] For refrigerators that use steel plates as door panels, when the door panels are filled with foaming material, the external force generated by the expansion of the foaming material during the foaming process will cause the door panels to deform. Usually before foaming, it is necessary to stick a piece of felt inside the door panel to prevent the door panel from deforming. At present, the felt used in most refrigerator steel plate doors is provided with a backing layer, a buffer layer and a barrier layer. Among them, the buffer material used to make the buffer layer is mainly made of PET chemical fiber or flame-retardant PET chemical fiber processed and bonded, which has poor elasticity and cannot completely absorb the expansion force of the foam glue during foaming, which may cause the refrigerator door panel to deform.

[0003] Poisson's ratio refers to the ratio of the transverse contraction strain to the longitudinal tensile strain when the material is subjected to unidirectional tension or compression. In most materials, the Poisson's ratio is usually positive, while negative Poisson's ratio materials refer to materials that expand in the transverse direction when stretched and contract in the transverse direction when compressed, which is mainly due to the special nature of their internal structure. Negative Poisson's ratio materials have unique advantages, such as high notch resistance, fracture resistance, high shear modulus, high resilience toughness and high energy absorption performance. If they can be introduced into the buffer layer of refrigerator door panels, it is expected to solve the problem of refrigerator door panel deformation. Summary of the invention

[0004] The object of the present invention is to provide a negative Poisson's ratio buffer material and a preparation process thereof, so as to solve the problem of poor elasticity of the buffer layer material of the refrigerator door panel in the background technology.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] In a first aspect, a negative Poisson's ratio cushioning material is composed of PE foam, wherein the PE foam comprises the following components by weight:

[0007] PE (polyethylene): 80-100 parts

[0008] Foaming agent: 5-10 parts

[0009] Dopamine modified porous wood powder: 10-25 parts

[0010] PTFE (polytetrafluoroethylene): 8-12 parts;

[0011] Zinc oxide: 2-4 parts;

[0012] The Poisson's ratio of the PE foam is -1 to 0.

[0013] The method for preparing the dopamine-modified porous wood powder comprises the following steps:

[0014] S1. Grind the straw into powder and add it to an acetic acid solution, reflux and stir at 130-140°C for 2-4h, and then collect the reaction product 1 by filtering; then add the reaction product 1 to a mixed solution of sodium hydroxide and sodium sulfate, reflux and stir at 90-100°C for 6-8h, filter, wash and dry to obtain porous wood powder;

[0015] S2. Add the porous wood powder and dopamine hydrochloride into a Tris-HCl buffer solution with a pH of 8 to 9, react at 45 to 55° C. for 1 to 2 hours, and then filter and collect the dopamine-modified porous wood powder.

[0016] Furthermore, the concentration of the acetic acid solution is 0.2-0.4 mol / L.

[0017] Furthermore, the mass percentage of the sodium hydroxide and sodium sulfate mixed solution is 8% to 12%, and the mass ratio of sodium hydroxide to sodium sulfate is 1:0.8.

[0018] Furthermore, the usage ratio of the straw to the acetic acid solution is 1 g:10 mL; the usage ratio of the reaction product 1 to the mixed solution of sodium hydroxide and sodium sulfate is 1 g:10 mL.

[0019] Furthermore, the stirring speed is 100 to 300 rpm.

[0020] Furthermore, the usage ratio of the porous wood powder, dopamine hydrochloride and Tris-HCl buffer solution is 1 g: 2-3 g: 100 mL.

[0021] Furthermore, the foaming agent is an amine derivative, and preferably, the foaming agent is azodicarbonamide (AC).

[0022] In a second aspect, a preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0023] The components are weighed according to the above weight proportions, and pre-mixed in a high-speed mixer for 10 to 20 minutes to fully mix the materials. The mixed materials are placed in a vacuum foaming device and foamed at 150 to 180° C. and a pressure of 8 to 10 MPa for 30 to 60 minutes. The temperature is then slowly lowered and the pressure is released to room temperature and pressure at a rate of 0.2 to 0.4° C. / min to obtain a negative Poisson's ratio cushioning material.

[0024] Beneficial effects of the present invention:

[0025] 1. The present invention provides a negative Poisson's ratio buffer material and a preparation process thereof. The negative Poisson's ratio buffer material is composed of PE foam. Dopamine-modified porous wood powder is prepared to improve the compatibility between polyethylene and polytetrafluoroethylene. At the same time, the dopamine-modified porous wood powder is used as a structural template to make polyethylene and polytetrafluoroethylene interlock with each other to form a two-dimensional concave hexagonal honeycomb structure with a significant negative Poisson's ratio effect. After testing, the tensile strength is ≥0.5MPa, the thickness is ≤1mm, the 25% compression rebound stress is ≤0.5MPa, and the surface impact absorption rate is ≥10%. The material is applied to the buffer layer of a refrigerator door panel to effectively improve the elasticity of the buffer layer, thereby further solving the problem of deformation of the refrigerator door panel.

[0026] 2. In the present invention, the straw cellulose in the straw powder is acetylated and converted into cellulose acetate by reacting with acetic acid. Then, under the action of the stabilizer sodium sulfate, the acetate group in the cellulose acetate is replaced by hydroxide, and a deacetylation reaction occurs, resulting in weight loss of the cellulose acetate. After washing with deionized water, the cellulose acetate becomes porous to realize the preparation of porous wood powder. Then, polydopamine is modified on the surface of the porous wood powder by oxidative self-polymerization of dopamine hydrochloride.

[0027] 3. Under normal conditions, polyethylene does not show negative Poisson's ratio characteristics after foaming. Polytetrafluoroethylene has good creep properties. By blending with polyethylene, due to the different creep properties of the two, the composite material can show negative Poisson's ratio characteristics. However, the melting point of polytetrafluoroethylene is 327°C, which is higher than that of polyethylene, resulting in poor compatibility with polyethylene. The acylation and deacylation reactions of straw are used to achieve weight loss and material pore formation, and then dopamine hydrochloride is used to self-polymerize and penetrate into the gaps to modify and form an elastic sponge structure, which is beneficial to Polydopamine has extremely strong surface adhesion properties and hydrogen bonds exist both between and within molecules, which can produce van der Waals forces with the polytetrafluoroethylene matrix to form mechanical interlocking. Under the action of hydrogen bonds, the polydopamine molecular chain will attract the end of the polytetrafluoroethylene chain, thereby obtaining a well-interlocked interface; on the other hand, dopamine-modified porous wood powder allows PTFE in-situ fiberization to produce more heterogeneous nucleation points. After fiber entanglement, the melt strength of PE is significantly increased, which limits the growth of bubbles and makes the bubble structure more fine and uniform. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The preparation method of dopamine-modified porous wood powder comprises the following steps:

[0030] S1. Grind the straw into powder and add it to 0.2-0.4 mol / L acetic acid solution, reflux and stir at 130-140°C and 100-300 rpm for 2-4 hours, and then filter and collect the reaction product 1; then add the reaction product 1 to a mixed solution of sodium hydroxide and sodium sulfate (m sodium hydroxide: m sodium sulfate = 1:0.8) with a mass percentage of 8-12%, reflux and stir at 90-100°C and 100-300 rpm for 6-8 hours, filter, wash and dry to obtain porous wood powder; the amount ratio of straw to acetic acid solution is 1g:10mL; the amount ratio of reaction product 1 to the mixed solution of sodium hydroxide and sodium sulfate is 1g:10mL;

[0031] S2. Add porous wood powder and dopamine hydrochloride into Tris-HCl buffer solution with pH=8-9, react at 45-55°C for 1-2 hours, and then filter and collect dopamine-modified porous wood powder. The dosage ratio of porous wood powder, dopamine hydrochloride and Tris-HCl buffer solution is 1g:2-3g:100mL.

[0032] A preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0033] The components are weighed according to the weight proportions of PE 80-100 parts, foaming agent 5-10 parts, dopamine modified porous wood powder 10-25 parts, PTFE 8-12 parts and zinc oxide 2-4 parts, and pre-mixed at a high speed of 400-600 rpm for 10-20 minutes in a high-speed mixer to fully mix the materials. The mixed materials are placed in a vacuum foaming device and foamed at 150-180° C. and a pressure of 8-10 MPa for 30-60 minutes. The temperature is then slowly lowered at a rate of 0.2-0.4° C. / min and the pressure is released to normal temperature and pressure to obtain a negative Poisson's ratio buffer material.

[0034] Example 1

[0035] The preparation method of dopamine-modified porous wood powder comprises the following steps:

[0036] S1. 10 g of straw was ground into powder and added to 100 mL of 0.3 mol / L acetic acid solution. The mixture was stirred under reflux at 135 ° C and 200 rpm for 3 h, and then the reaction product 1 was collected by filtration; 10 g of the reaction product 1 was added to 100 mL of a 10% mixed solution of sodium hydroxide and sodium sulfate (m sodium hydroxide: m sodium sulfate = 1:0.8) at 95 ° C and 200 rpm for 7 h, and then filtered, washed and dried to obtain porous wood powder;

[0037] S2. Add 10 g of porous wood powder and 25 g of dopamine hydrochloride into 1000 mL of Tris-HCl buffer solution with a pH of 8.5, react at 50° C. for 1.5 h, and then filter and collect the dopamine-modified porous wood powder.

[0038] Example 2

[0039] A preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0040] The components were weighed according to the weight proportions of 90 parts of PE, 8 parts of azodicarbonamide, 18 parts of dopamine-modified porous wood powder, 10 parts of PTFE and 3 parts of zinc oxide, and pre-mixed at a high speed of 500 rpm for 15 minutes in a high-speed mixer to fully mix the materials. The mixed materials were placed in a vacuum foaming device and foamed at 165° C. and a pressure of 9 MPa for 45 minutes. The temperature was then slowly lowered at a rate of 0.3° C. / min and the pressure was released to room temperature and pressure to obtain a negative Poisson's ratio buffer material.

[0041] Example 3

[0042] A preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0043] The components were weighed according to the weight proportions of 80 parts of PE, 8 parts of azodicarbonamide, 10 parts of dopamine-modified porous wood powder, 8 parts of PTFE and 3 parts of zinc oxide, and pre-mixed at a high speed of 500 rpm for 15 minutes in a high-speed mixer to fully mix the materials. The mixed materials were placed in a vacuum foaming device and foamed at 165° C. and a pressure of 9 MPa for 45 minutes. The temperature was then slowly lowered at a rate of 0.3° C. / min and the pressure was released to room temperature and pressure to obtain a negative Poisson's ratio buffer material.

[0044] Example 4

[0045] A preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0046] The components were weighed according to the weight proportions of 100 parts of PE, 8 parts of azodicarbonamide, 25 parts of dopamine-modified porous wood powder, 12 parts of PTFE and 3 parts of zinc oxide, and pre-mixed at a high speed of 500 rpm for 15 minutes in a high-speed mixer to fully mix the materials. The mixed materials were placed in a vacuum foaming device and foamed at 165° C. and a pressure of 9 MPa for 45 minutes. The temperature was then slowly lowered at a rate of 0.3° C. / min and the pressure was released to room temperature and pressure to obtain a negative Poisson's ratio buffer material.

[0047] Comparative Example 1

[0048] A preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0049] 10 g of straw was ground into powder and added into 100 mL of 0.3 mol / L acetic acid solution, and the mixture was refluxed and stirred at 135° C. and 200 rpm for 3 h, and then the reaction product 1 was collected by filtration; 10 g of the reaction product 1 was added into 100 mL of a 10% by mass sodium hydroxide and sodium sulfate mixed solution (m sodium hydroxide: m sodium sulfate = 1:0.8), and the mixture was refluxed and stirred at 95° C. and 200 rpm for 7 h, and then the porous wood powder was obtained by filtration, washing and drying;

[0050] The components were weighed according to the weight proportions of 90 parts of PE, 8 parts of azodicarbonamide, 18 parts of porous wood powder, 10 parts of PTFE and 3 parts of zinc oxide, and pre-mixed at a high speed of 500 rpm for 15 minutes in a high-speed mixer to fully mix the materials. The mixed materials were placed in a vacuum foaming device and foamed at 165° C. and a pressure of 9 MPa for 45 minutes. The temperature was then slowly lowered at a rate of 0.3° C. / min and the pressure was released to room temperature and pressure to obtain a negative Poisson's ratio cushioning material.

[0051] Comparative Example 2

[0052] A preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0053] 10 g of straw was ground into powder and 25 g of dopamine hydrochloride was added into 1000 mL of Tris-HCl buffer solution with pH = 8.5, and the mixture was reacted at 50°C for 1.5 h, and then the dopamine-modified wood powder was collected by filtration;

[0054] The components were weighed according to the weight proportions of 90 parts of PE, 8 parts of azodicarbonamide, 18 parts of dopamine-modified wood powder, 10 parts of PTFE and 3 parts of zinc oxide, and pre-mixed at a high speed of 500 rpm for 15 minutes in a high-speed mixer to fully mix the materials. The mixed materials were placed in a vacuum foaming device and foamed at 165° C. and a pressure of 9 MPa for 45 minutes. The temperature was then slowly lowered at a rate of 0.3° C. / min and the pressure was released to room temperature and pressure to obtain a negative Poisson's ratio buffer material.

[0055] Comparative Example 3

[0056] A preparation process of a negative Poisson's ratio buffer material comprises the following steps:

[0057] The components were weighed according to the weight proportions of 90 parts of PE, 8 parts of azodicarbonamide, 6 parts of porous wood powder, 9 parts of dopamine hydrochloride, 10 parts of PTFE and 3 parts of zinc oxide, and pre-mixed at a high speed of 500 rpm for 15 minutes in a high-speed mixer to fully mix the materials. The mixed materials were placed in a vacuum foaming device and foamed at 165° C. and a pressure of 9 MPa for 45 minutes. The temperature was then slowly lowered at a rate of 0.3° C. / min and the pressure was released to room temperature and pressure to obtain a negative Poisson's ratio buffer material.

[0058] Comparative Example 4

[0059] The difference from Example 2 is that 10 parts of PTFE are not added to the components, but are replaced by an equal amount of PE.

[0060] Comparative Example 5

[0061] The difference from Example 2 is that 10 parts of dopamine-modified porous wood powder are not added to the components, but are replaced by an equal amount of PE.

[0062] Comparative Example 6

[0063] The difference from Example 2 is that 10 parts of dopamine-modified porous wood powder and 10 parts of PTFE are not added to the components, but are replaced by an equal amount of PE.

[0064] The surface layer and the inner layer of the buffer material prepared in Examples 2 to 4 and Comparative Examples 1 to 6 were subjected to a Poisson's ratio test according to GB / T1040.1-2006 standard, and a rebound recovery test was performed using a WTT-5 impact elasticity tester to observe the percentage of pendulum rebound. Each group was tested 3 times and the average value was taken. The test results are shown in Table 1:

[0065] Table 1

[0066]

[0067]

[0068] As can be seen from Table 1, the present invention improves the compatibility between polyethylene and polytetrafluoroethylene by preparing dopamine-modified porous wood powder. At the same time, it serves as a structural template to make polyethylene and polytetrafluoroethylene interlock with each other to form a two-dimensional concave hexagonal honeycomb structure with a significant negative Poisson's ratio effect, and the ratio of the inner layer to the surface layer is almost the same, indicating that its structure is stable; in Comparative Example 1, the porous wood powder has a low surface hydroxyl content without dopamine modification, and its ability to regulate the compatibility between PE and PTFE is slightly weak; in Comparative Example 2, the wood powder has not been subjected to pore-forming treatment, and the internal gas of the PE material is difficult to be effectively conducted through the pores during the foaming process, resulting in unstable negative Poisson's ratio characteristics of the surface and the interior of the foam material; in Comparative Example 3, although porous wood powder and dopamine hydrochloride are added, cross-linking between dopamine and porous wood powder is not achieved, and good negative Poisson's ratio performance cannot be formed; in addition, it can be seen from Comparative Examples 4 to 6 that dopamine-modified porous wood powder has a certain ability to synergistically improve the elasticity and negative Poisson's ratio of PE foam.

[0069] The negative Poisson's ratio buffer material prepared by the present invention has good resilience performance. The material is applied to the buffer layer of the refrigerator door panel, which can effectively improve the elasticity of the buffer layer, thereby further solving the problem of refrigerator door panel deformation.

[0070] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or includes elements inherent to such process, method, article or device.

[0071] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A negative Poisson's ratio cushioning material, composed of PE foam, characterized in that: The PE foam comprises the following components in parts by mass: PE: 80-100 copies; Foaming agent: 5-10 parts; Dopamine modified porous wood powder: 10-25 parts; PTFE: 8-12 parts; Zinc oxide: 2-4 parts; The Poisson's ratio of the PE foam is -1 to 0.

2. A negative Poisson's ratio cushioning material according to claim 1, characterized in that: The method for preparing the dopamine-modified porous wood powder comprises the following steps: S1. Grind the straw into powder and add it to an acetic acid solution, reflux and stir at 130-140°C for 2-4h, and then collect the reaction product 1 by filtering; then add the reaction product 1 to a mixed solution of sodium hydroxide and sodium sulfate, reflux and stir at 90-100°C for 6-8h, filter, wash and dry to obtain porous wood powder; S2. Add the porous wood powder and dopamine hydrochloride into a Tris-HCl buffer solution with a pH of 8 to 9, react at 45 to 55° C. for 1 to 2 hours, and then filter and collect the dopamine-modified porous wood powder.

3. A negative Poisson's ratio cushioning material according to claim 2, characterized in that: The concentration of the acetic acid solution is 0.2-0.4 mol / L.

4. A negative Poisson's ratio cushioning material according to claim 2, characterized in that: The mass percentage of the sodium hydroxide and sodium sulfate mixed solution is 8% to 12%, and the mass ratio of sodium hydroxide to sodium sulfate is 1:0.

8.

5. A negative Poisson's ratio cushioning material according to claim 2, characterized in that: The dosage ratio of the straw to the acetic acid solution is 1 g:10 mL; the dosage ratio of the reaction product 1 to the mixed solution of sodium hydroxide and sodium sulfate is 1 g:10 mL.

6. A negative Poisson's ratio cushioning material according to claim 2, characterized in that: The usage ratio of the porous wood powder, dopamine hydrochloride and Tris-HCl buffer solution is 1g: 2-3g: 100mL.

7. A negative Poisson's ratio cushioning material according to claim 1, characterized in that: The foaming agent is an amine derivative.

8. A process for preparing a negative Poisson's ratio buffer material according to any one of claims 1 to 7, characterized in that: The following steps are involved: The components are weighed according to the above weight proportions, pre-mixed in a mixer for 10 to 20 minutes to fully mix the materials, and the mixed materials are placed in a vacuum foaming device for foaming at 150 to 180° C. and a pressure of 8 to 10 MPa for 30 to 60 minutes. Thereafter, the temperature is slowly lowered at a rate of 0.2 to 0.4° C. / min and the pressure is released to normal temperature and pressure to obtain a negative Poisson's ratio cushioning material.