Flame-retardant cable material with high volume resistivity and preparation method thereof
The filling agent is prepared through esterification and polycondensation reaction, combined with catalyst and twin screw extrusion technology, and the problem of volume resistivity of cable materials decreased in rainy weather, improved mechanical properties and water resistance, and extended the service life of the cable .
Patent Information
- Application Number
- CN202411135025.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The volume resistivity of existing cable materials has severely decreased in long-term rainy weather and poor water barrier performance, resulting in frequent maintenance.
Fillers are prepared by esterification and polycondensation reaction, including refined terephthalic acid, ethylene glycol and silicone reagents, and catalyst antimony trioxide is added, and melted and kneaded through a twin-screw extruder to produce a high volume resistivity resistance. Burn cable material.
It improves the mechanical properties and water resistance of cable materials, stabilizes the volume resistivity, reduces the decrease in conductivity after long-term immersion, and extends the service life of the cable.
Smart Images

Figure BDA0004999152730000021 
Figure BDA0004999152730000022 
Figure BDA0004999152730000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cable materials, and in particular to a flame-retardant cable material with high volume resistivity and a preparation method thereof. Background Art
[0002] Wires, cables and optical cables are mainly responsible for energy and information transmission and are an indispensable part of daily life. At present, the output value of the cable industry exceeds one trillion yuan, making it one of the largest supporting industries in the entire economic system and the second largest industry after the automotive industry.
[0003] Cable materials are generally divided into polyethylene (PE) cable materials and polyvinyl chloride (PVC) cable materials. Polyethylene (PE) cable materials have a high plasticizing temperature. If the processing technology is improper, surface defects will occur, which may easily cause problems such as cracking of the cable during storage and use. PVC cable materials have the characteristics of high strength, high temperature cracking resistance, low thermal deformation and good flame retardancy. At the same time, they have good processing performance and low production cost.
[0004] However, the volume resistivity of existing cable materials decreases significantly during long periods of rainy weather, and they may often need to be repaired due to poor water-blocking properties.
[0005] For example, CN116656026A discloses a water-tree resistant cross-linked polyethylene cable material, comprising polyethylene, modified SiO 2 Nanofiller, vinyl trimethoxysilane, crosslinking agent and antioxidant, wherein the modified SiO2 nanofiller is modified by heptadecafluorodecyl trimethoxysilane to form SiO 2 The invention discloses a method for preparing a water-tree resistant cross-linked polyethylene cable material, and obtains a water-tree resistant cross-linked polyethylene cable material with excellent mechanical properties, thermal stability and water-tree resistant performance through a three-step method; the invention finally discloses an application of a water-tree resistant cross-linked polyethylene cable material in a cable, and the cable obtained by extruding and directly coating the water-tree resistant cross-linked polyethylene cable material on a wire core has better safety and stability.
[0006] For example, CN116285089A discloses a water-blocking low-smoke halogen-free flame-retardant cable material and its preparation method, which belongs to the technical field of cable materials, and includes the following raw materials by weight: 100 parts of polyolefin resin, 28-30 parts of flame-retardant filler, 8-12 parts of unsaturated coupling agent, 0.13-0.15 parts of cross-linking agent, 0.04-0.05 parts of antioxidant, 5-6 parts of compatibilizer, 0.3-0.4 parts of catalyst; polyolefin resin and unsaturated coupling agent are mixed to obtain base material, and then the base material, flame-retardant filler, cross-linking agent and compatibilizer are banburyed, and finally antioxidant and catalyst are added, extruded and filmed, and placed under natural conditions for 72 hours. In the present invention, polyolefin resin is used as cable insulation material, and magnesium hydroxide and aluminum hydroxide in inorganic flame retardant are added as inorganic flame retardant to improve flame retardant performance, unsaturated coupling agent is added to improve processing performance of raw materials, and the addition amount of inorganic flame retardant is reduced.
[0007] However, the actual water-blocking performance of the above materials has not been tested, and the volume resistivity decreases significantly after a long period of rainy weather. Therefore, a flame-retardant cable material with high volume resistivity is urgently needed. Summary of the invention
[0008] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a flame-retardant cable material with high volume resistivity and a preparation method thereof. The cable material provided in the present application has excellent mechanical properties, high volume resistivity and limited decrease in volume conductivity after long-term immersion in water.
[0009] The purpose of the present invention can be achieved by the following technical solutions:
[0010] The present invention provides a flame-retardant cable material with high volume resistivity, comprising the following components in parts by weight:
[0011]
[0012] The filler is prepared in the following manner:
[0013] The mixed purified terephthalic acid and ethylene glycol are subjected to esterification reaction, and after the esterification is completed, an organosilicon reagent is added to carry out polycondensation reaction to obtain a filler.
[0014] Preferably, the flame retardant cable material comprises the following components in parts by weight:
[0015]
[0016] Preferably, the esterification reaction and polycondensation reaction are carried out in a reaction kettle;
[0017] and / or, the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent is 1:(1-1.5):(1-1.5);
[0018] And / or, the organosilicon reagent at least includes the compound described in the following formula (1):
[0019]
[0020] In the formula, R is a C0-C20 saturated alkyl group,
[0021] R 1 and R 2 are the same or different and are each independently selected from phenyl or C1-C10 straight chain alkyl,
[0022] X is selected from O or NH,
[0023] m is a positive integer;
[0024] And / or, the esterification reaction further requires the addition of a catalyst, the catalyst is preferably antimony trioxide, and the addition amount of antimony trioxide is 400-600 ppm;
[0025] And / or, the reaction temperature of the esterification reaction is 240-260°C;
[0026] and / or, when the water output of the esterification reaction reaches 90% of the theoretical water output, stopping the esterification reaction;
[0027] And / or, after adding the organosilicon reagent, react at normal pressure for 0.5 to 1 hour, and then perform a pre-condensation treatment. The specific reaction conditions of the pre-condensation reaction are: slowly evacuate to 80 to 100 Pa within 1 to 3 hours, then raise the temperature of the entire system to 270 to 300° C., and react for 1 to 3 hours.
[0028] Preferably, the stabilizer is a mixture of one or more of lead stearate, barium stearate, barium laurate, zinc stearate, tribasic lead sulfate, dibasic lead phosphite, dibasic lead phthalate, lead silicate, lead cyanurate, and calcium stearate;
[0029] And / or, the flame retardant is one or more combinations of antimony trioxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, and montmorillonite;
[0030] And / or, the lubricant is one or more combinations of liquid paraffin, natural paraffin, microcrystalline paraffin, polyethylene wax, and stearic acid;
[0031] And / or, the plasticizer is one or more combinations of dioctyl phthalate, tricresyl phosphate, diisononyl phthalate, dioctyl terephthalate, and trioctyl terephthalate.
[0032] The present invention also provides a method for preparing a flame-retardant cable material with high volume resistivity, comprising the following steps:
[0033] The polyvinyl chloride, stabilizer and plasticizer are mixed by high-speed stirring, and the first mixture is obtained after heating. Then, the mixture is switched to low-speed mixing and fillers, flame retardants and lubricants are added in sequence to obtain a second mixture. After the second mixture is cooled, it is put into a twin-screw extruder for melt kneading and extrusion, extrusion cooling, and pellets are obtained to obtain a cable material.
[0034] Preferably, the high-speed stirring and mixing rate is 700-1000 rpm, and the high-speed stirring time is 20-60 min;
[0035] And / or, the heating specifically comprises the following steps: heating to 90-100° C. at a rate of 5-8° C. / min;
[0036] And / or, the low-speed mixing rate is 150 rpm-200 rpm, and the low-speed mixing time is 200-300 s;
[0037] And / or, the flame retardant cable material comprises the following components in parts by weight: 100-150 parts of polyvinyl chloride, 5-15 parts of stabilizer, 20-50 parts of filler, 20-40 parts of flame retardant, 1-3 parts of lubricant, and 30-50 parts of plasticizer.
[0038] Preferably, the filler is prepared in the following manner:
[0039] The mixed purified terephthalic acid and ethylene glycol are subjected to esterification reaction, and after the esterification is completed, an organosilicon reagent is added to carry out polycondensation reaction to obtain a filler.
[0040] Preferably, the esterification reaction and polycondensation reaction are carried out in a reaction kettle;
[0041] and / or, the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent is 1:(1-1.5):(1-1.5);
[0042] And / or, the organosilicon reagent at least includes the compound described in the following formula (1):
[0043]
[0044] In the formula, R is a C0-C20 saturated alkyl group,
[0045] R 1 and R 2 are the same or different and are each independently selected from phenyl or C1-C10 straight chain alkyl,
[0046] X is selected from O or NH,
[0047] m is a positive integer;
[0048] And / or, the esterification reaction further requires the addition of a catalyst, the catalyst is preferably antimony trioxide, and the addition amount of antimony trioxide is 400-600 ppm;
[0049] And / or, the reaction temperature of the esterification reaction is 240-260°C;
[0050] and / or, when the water output of the esterification reaction reaches 90% of the theoretical water output, stopping the esterification reaction;
[0051] And / or, after adding the organosilicon reagent, react at normal pressure for 0.5 to 1 hour, and then perform a pre-condensation treatment. The specific reaction conditions of the pre-condensation reaction are: slowly evacuate to 80 to 100 Pa within 1 to 3 hours, then raise the temperature of the entire system to 270 to 300° C., and react for 1 to 3 hours.
[0052] Preferably, the stabilizer is a mixture of one or more of lead stearate, barium stearate, barium laurate, zinc stearate, tribasic lead sulfate, dibasic lead phosphite, dibasic lead phthalate, lead silicate, lead cyanurate, and calcium stearate;
[0053] And / or, the flame retardant is one or more combinations of antimony trioxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, and montmorillonite,
[0054] And / or, the lubricant is one or more combinations of liquid paraffin, natural paraffin, microcrystalline paraffin, polyethylene wax, and stearic acid;
[0055] And / or, the plasticizer is one or more combinations of dioctyl phthalate, tricresyl phosphate, diisononyl phthalate, dioctyl terephthalate, and trioctyl terephthalate.
[0056] The present invention further provides a cable material obtained by the preparation method of the flame-retardant cable material with high volume resistivity as described above.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] 1. Compared with the prior art, the flame retardant in this application can improve compatibility, enhance interfacial bonding, and effectively transfer stress through interfacial bonding, thereby improving mechanical properties. In addition, the filler provided in this application is a polar polymer, whose active groups interact with the energy groups on the flame retardant, and whose molecular chains can be combined with the flame retardant through physical entanglement and van der Waals forces, thereby improving the interfacial adhesion between the various components of the cable material, thereby improving the mechanical properties of the cable material.
[0059] 2. Compared with the prior art, the filler used in the present application has a weakened interaction with the polyvinyl chloride macromolecular chain, and its active groups interact with the flame retardant's upper energy groups. Its molecular chains can be combined with the flame retardant through physical entanglement and van der Waals forces to make its structure compact, so that the intermolecular force between polyvinyl chloride and the filler is weakened, thereby increasing the activation energy of ion migration, reducing ion activity, and improving volume resistivity. In addition, the filler used in the present application has a strong hydrophobic property, which increases the water-blocking property of the cable material, thereby reducing the volume resistivity of the cable material. DETAILED DESCRIPTION
[0060] For ease of understanding of the present application, the present application will be described more fully below by way of embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0061] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.
[0062] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art in the technical field of the present application. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. It should be noted that, unless otherwise specified, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" include the number, and the meaning of "multiple" in "one or more" is more than two.
[0063] The volume resistivity of existing cable materials decreases significantly during long periods of rainy weather, and they may often need to be repaired due to poor water-blocking performance.
[0064] Based on this, the first aspect of the embodiment of the present application provides a flame-retardant cable material with high volume resistivity, including the following components in parts by weight:
[0065]
[0066] The filler is prepared in the following manner:
[0067] The mixed purified terephthalic acid and ethylene glycol are subjected to esterification reaction, and after the esterification is completed, an organosilicon reagent is added to carry out polycondensation reaction to obtain a filler.
[0068] In some optional embodiments, the flame retardant cable material comprises the following components in parts by weight:
[0069]
[0070]
[0071] In a preferred embodiment, the flame retardant cable material comprises the following components in parts by weight:
[0072]
[0073] In some optional embodiments, the esterification reaction and the polycondensation reaction are carried out in a reactor, and the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent is 1:(1-1.5):(1-1.5). Of course, those skilled in the art should know that the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent can be 1:1:1, 1:1:1.1, 1:1:1.2, 1:1:1.3, 1:1:1.4, 1:1:1.5, 1:1.1:1, 1:1.1:1.1, 1:1.1:1.2, 1:1.1:1.3, 1:1.1:1.4, 1:1.1:1.5, 1:1.2:1, 1:1.2: 1.1, 1:1.2:1.2, 1:1.2:1.3, 1:1.2:1.4, 1:1.2:1.5, 1:1.3:1, 1:1.3:1.1, 1:1.3:1.2, 1:1.3:1.4, 1:1.3:1.5, 1:1.4:1, 1:1.4:1.1, 1:1.4:1.2, 1:1.4:1.3, 1:1.4:1.4, 1:1.4:1.5, 1:1.5:1, 1:1.5:1.1, 1:1.5:1.2, 1:1.5:1.3, 1:1.5:1.4, 1:1.5:1.5 or any value within the above range, preferably 1:1.3:1.5.
[0074] In some optional embodiments, the organosilicon reagent includes at least a compound of the following formula (1):
[0075]
[0076] Wherein, R is a C0-C20 saturated alkyl group;
[0077] R1 and R2 are the same or different and are each independently selected from phenyl or C1-C10 straight chain alkyl;
[0078] X is selected from O or NH;
[0079] m is a positive integer.
[0080] In some optional embodiments, the esterification reaction further requires the addition of a catalyst, and the catalyst is preferably antimony trioxide, and the amount of antimony trioxide added is 400-600 ppm. Of course, those skilled in the art should be aware that the amount of antimony trioxide added can be 400 ppm, 450 ppm, 500 ppm, 550 ppm, 600 ppm or any value within the above range, preferably 500 ppm.
[0081] In particular, in some optional embodiments, the reaction conditions need to be controlled during the esterification reaction to accelerate the reaction rate. In this embodiment, the reaction temperature of the esterification reaction is 240-260°C, preferably 250°C, and the time of the esterification reaction is not specially set. Preferably, the esterification reaction is stopped when the water output of the esterification reaction reaches 90% of the theoretical water output.
[0082] In addition, after the esterification reaction is completed, an organosilicon reagent is added to carry out a condensation reaction. In some optional embodiments, after the addition of the organosilicon reagent, the reaction is first carried out at normal pressure for 0.5 to 1 hour, preferably 0.5 hours, and then a pre-condensation treatment is carried out. The specific reaction conditions of the pre-condensation reaction are: slowly evacuating to 80 to 100 Pa within 1 to 3 hours, preferably, slowly evacuating to 100 Pa within 1.5 hours.
[0083] In some optional embodiments, after the pre-polycondensation reaction is completed, the temperature of the entire system is raised to 270-300° C., preferably 270-280° C. for polycondensation reaction, and the reaction time is 1-3 hours, preferably 1.5 hours.
[0084] In some optional embodiments, the stabilizer is a mixture of one or more of lead stearate, barium stearate, barium laurate, zinc stearate, tribasic lead sulfate, dibasic lead phosphite, dibasic lead phthalate, lead silicate, lead cyanurate, and calcium stearate, preferably a calcium zinc stabilizer mixed with lead stearate and zinc stearate.
[0085] In some optional embodiments, the flame retardant is one or more combinations of antimony trioxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, and montmorillonite, preferably a mixture of aluminum hydroxide, hydrotalcite, and montmorillonite. The specific mixing ratio is not limited in this application.
[0086] In some optional embodiments, the lubricant is one or more combinations of liquid paraffin, natural paraffin, microcrystalline paraffin, polyethylene wax, and stearic acid. Preferably, the lubricant is polyethylene wax and its melting point is 115° C. to 120° C.;
[0087] In some optional embodiments, the plasticizer is one or more combinations of dioctyl phthalate, tricresyl phosphate, diisononyl phthalate, dioctyl terephthalate, and trioctyl terephthalate, preferably dioctyl phthalate.
[0088] A second aspect of the embodiments of the present application provides a method for preparing a flame-retardant cable material with high volume resistivity, comprising the following steps:
[0089] The polyvinyl chloride, stabilizer and plasticizer are mixed by high-speed stirring, and the first mixture is obtained after heating. Then, the mixture is switched to low-speed mixing and fillers, flame retardants and lubricants are added in sequence to obtain a second mixture. After the second mixture is cooled, it is put into a twin-screw extruder for melt kneading and extrusion, extrusion cooling, and pellets are obtained to obtain a cable material.
[0090] In some optional embodiments, the high-speed stirring and mixing rate is 700-1000rpm, preferably 800rpm, and the high-speed stirring time is 20-60min, preferably 20min; the heating specifically includes the following steps: heating to 90-100℃ at a rate of 5-8℃ / min, preferably heating to 100℃ at a rate of 5℃ / min; the low-speed mixing rate is 150rpm-200rpm, preferably 180rpm, and the low-speed mixing time is 200-300s, preferably 240s; the cooling to a temperature of 45-60℃.
[0091] In some optional embodiments, the flame retardant cable material includes the following components by weight: 100-150 parts of polyvinyl chloride, 5-15 parts of stabilizer, 20-50 parts of filler, 20-40 parts of flame retardant, 1-3 parts of lubricant, and 30-50 parts of plasticizer, preferably: 100-140 parts of polyvinyl chloride, 8-12 parts of stabilizer, 30-50 parts of filler, 30-40 parts of flame retardant, 1.5-3 parts of lubricant, and 40-50 parts of plasticizer.
[0092] In some optional embodiments, the filler is prepared in the following manner:
[0093] The mixed purified terephthalic acid and ethylene glycol are subjected to esterification reaction, and after the esterification is completed, an organosilicon reagent is added to carry out polycondensation reaction to obtain a filler.
[0094] In some optional embodiments, the esterification reaction and the polycondensation reaction are carried out in a reactor, and the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent is 1:(1-1.5):(1-1.5). Of course, those skilled in the art should know that the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent can be 1:1:1, 1:1:1.1, 1:1:1.2, 1:1:1.3, 1:1:1.4, 1:1:1.5, 1:1.1:1, 1:1.1:1.1, 1:1.1:1.2, 1:1.1:1.3, 1:1.1:1.4, 1:1.1:1.5, 1:1.2:1, 1:1.2: 1.1, 1:1.2:1.2, 1:1.2:1.3, 1:1.2:1.4, 1:1.2:1.5, 1:1.3:1, 1:1.3:1.1, 1:1.3:1.2, 1:1.3:1.4, 1:1.3:1.5, 1:1.4:1, 1:1.4:1.1, 1:1.4:1.2, 1:1.4:1.3, 1:1.4:1.4, 1:1.4:1.5, 1:1.5:1, 1:1.5:1.1, 1:1.5:1.2, 1:1.5:1.3, 1:1.5:1.4, 1:1.5:1.5 or any value within the above range, preferably 1:1.3:1.5.
[0095] In some optional embodiments, the organosilicon reagent includes at least a compound of the following formula (1):
[0096]
[0097] Wherein, R is a C0-C20 saturated alkyl group;
[0098] R 1 and R 2 are the same or different and are each independently selected from phenyl or C1-C10 straight chain alkyl;
[0099] X is selected from O or NH;
[0100] m is a positive integer.
[0101] In some optional embodiments, the esterification reaction further requires the addition of a catalyst, and the catalyst is preferably antimony trioxide, and the amount of antimony trioxide added is 400-600 ppm. Of course, those skilled in the art should be aware that the amount of antimony trioxide added can be 400 ppm, 450 ppm, 500 ppm, 550 ppm, 600 ppm or any value within the above range, preferably 500 ppm.
[0102] In particular, in some optional embodiments, the reaction conditions need to be controlled during the esterification reaction to accelerate the reaction rate. In this embodiment, the reaction temperature of the esterification reaction is 240-260°C, preferably 250°C, and the time of the esterification reaction is not specially set. Preferably, the esterification reaction is stopped when the water output of the esterification reaction reaches 90% of the theoretical water output.
[0103] In addition, after the esterification reaction is completed, an organosilicon reagent is added to carry out a condensation reaction. In some optional embodiments, after the addition of the organosilicon reagent, the reaction is first carried out at normal pressure for 0.5 to 1 hour, preferably 0.5 hours, and then a pre-condensation treatment is carried out. The specific reaction conditions of the pre-condensation reaction are: slowly evacuating to 80 to 100 Pa within 1 to 3 hours, preferably, slowly evacuating to 100 Pa within 1.5 hours.
[0104] In some optional embodiments, after the pre-polycondensation reaction is completed, the temperature of the entire system is raised to 270-300° C., preferably 270-280° C. for polycondensation reaction, and the reaction time is 1-3 hours, preferably 1.5 hours.
[0105] In some optional embodiments, the stabilizer is a mixture of one or more of lead stearate, barium stearate, barium laurate, zinc stearate, tribasic lead sulfate, dibasic lead phosphite, dibasic lead phthalate, lead silicate, lead cyanurate, and calcium stearate, preferably a calcium zinc stabilizer mixed with lead stearate and zinc stearate; the flame retardant is a combination of one or more of antimony trioxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, and montmorillonite, preferably aluminum hydroxide, hydrotalcite, and montmorillonite. The mixture of de-earthed materials, the specific mixing ratio is not limited in the present application; the lubricant includes one or more combinations of liquid paraffin, natural paraffin, microcrystalline paraffin, polyethylene wax, and stearic acid. Preferably, the lubricant is polyethylene wax and its melting point is 115°C to 120°C; the plasticizer is one or more combinations of dioctyl phthalate, tricresyl phosphate, diisononyl phthalate, dioctyl terephthalate, and trioctyl phthalate, preferably dioctyl phthalate.
[0106] The above implementation is described in more detail below in conjunction with specific examples.
[0107] Example 1
[0108] This embodiment provides a flame-retardant cable material with high volume resistivity, and the preparation method thereof is as follows:
[0109] The polyvinyl chloride, stabilizer and plasticizer were stirred and mixed at 800 rpm for 20 minutes and the temperature was raised to 100° C. at a rate of 5° C. / min at the same time. Then, the mixture was switched to low-speed mixing at 180 rpm and fillers, flame retardants and lubricants were added in sequence. The mixture was mixed at low speed for 240 seconds to obtain a second mixture. After the second mixture was cooled, it was put into a twin-screw extruder for melt kneading and extrusion. The mixture was extruded and cooled to prepare pellets to obtain a cable material.
[0110] The mass ratio of polyvinyl chloride, stabilizer, filler, flame retardant, lubricant and plasticizer is 120:10:50:35:2:40. The stabilizer is calcium zinc stabilizer, the plasticizer is dioctyl phthalate, the flame retardant is a mixture of aluminum hydroxide, hydrotalcite and montmorillonite in a mass ratio of 40:40:10, and the lubricant is polyethylene wax with a melting point of 115°C to 120°C.
[0111] The filler is prepared in the following manner:
[0112] Purified terephthalic acid and ethylene glycol were mixed and antimony trioxide was added as a catalyst to carry out esterification reaction. The reaction temperature was 250°C. When the water output of the esterification reaction reached 90% of the theoretical water output, the esterification reaction was stopped. After the esterification was completed, an organosilicon reagent was added to carry out polycondensation reaction. The reaction was first carried out at normal pressure for 0.5h, and then the vacuum was slowly evacuated to 100 Pa within 1.5h. The temperature of the whole system was then raised to 280°C and reacted for 1.5h to obtain a filler, wherein the organosilicon reagent includes the following structure:
[0113]
[0114] Example 2
[0115] This embodiment provides a flame-retardant cable material with high volume resistivity, and the preparation method thereof is as follows:
[0116] The polyvinyl chloride, stabilizer and plasticizer were stirred and mixed at 800 rpm for 20 minutes and the temperature was raised to 100° C. at a rate of 5° C. / min at the same time. Then, the mixture was switched to low-speed mixing at 180 rpm and fillers, flame retardants and lubricants were added in sequence. The mixture was mixed at low speed for 240 seconds to obtain a second mixture. After the second mixture was cooled, it was put into a twin-screw extruder for melt kneading and extrusion. The mixture was extruded and cooled to prepare pellets to obtain a cable material.
[0117] The mass ratio of polyvinyl chloride, stabilizer, filler, flame retardant, lubricant and plasticizer is 120:10:50:35:2:40. The stabilizer is calcium zinc stabilizer, the plasticizer is dioctyl phthalate, the flame retardant is a mixture of aluminum hydroxide, hydrotalcite and montmorillonite in a mass ratio of 40:40:10, and the lubricant is polyethylene wax with a melting point of 115°C to 120°C.
[0118] The filler is prepared in the following manner:
[0119] Purified terephthalic acid and ethylene glycol were mixed and antimony trioxide was added as a catalyst to carry out esterification reaction. The reaction temperature was 250°C. When the water output of the esterification reaction reached 90% of the theoretical water output, the esterification reaction was stopped. After the esterification was completed, an organosilicon reagent was added to carry out polycondensation reaction. The reaction was first carried out at normal pressure for 0.5h, and then the vacuum was slowly evacuated to 100 Pa within 1.5h. The temperature of the whole system was then raised to 280°C and reacted for 1.5h to obtain a filler, wherein the organosilicon reagent includes the following structure:
[0120]
[0121] Example 3
[0122] This embodiment provides a flame-retardant cable material with high volume resistivity, and the preparation method thereof is as follows:
[0123] The polyvinyl chloride, stabilizer and plasticizer were stirred and mixed at 800 rpm for 20 minutes and the temperature was raised to 100° C. at a rate of 5° C. / min at the same time. Then, the mixture was switched to low-speed mixing at 180 rpm and fillers, flame retardants and lubricants were added in sequence. The mixture was mixed at low speed for 240 seconds to obtain a second mixture. After the second mixture was cooled, it was put into a twin-screw extruder for melt kneading and extrusion. The mixture was extruded and cooled to prepare pellets to obtain a cable material.
[0124] The mass ratio of polyvinyl chloride, stabilizer, filler, flame retardant, lubricant and plasticizer is 120:10:50:35:2:40. In addition, the stabilizer is lead stearate, the plasticizer is dioctyl phthalate, the flame retardant is a mixture of aluminum hydroxide, hydrotalcite and montmorillonite in a mass ratio of 40:40:10, and the lubricant is polyethylene wax with a melting point of 115°C to 120°C.
[0125] The filler is prepared in the following manner:
[0126] Purified terephthalic acid and ethylene glycol were mixed and antimony trioxide was added as a catalyst to carry out esterification reaction. The reaction temperature was 250°C. When the water output of the esterification reaction reached 90% of the theoretical water output, the esterification reaction was stopped. After the esterification was completed, an organosilicon reagent was added to carry out polycondensation reaction. The reaction was first carried out at normal pressure for 0.5h, and then the vacuum was slowly evacuated to 100 Pa within 1.5h. The temperature of the whole system was then raised to 280°C and reacted for 1.5h to obtain a filler, wherein the organosilicon reagent includes the following structure:
[0127]
[0128] Example 4
[0129] This embodiment provides a flame-retardant cable material with high volume resistivity, and the preparation method thereof is as follows:
[0130] The polyvinyl chloride, stabilizer and plasticizer were stirred and mixed at 800 rpm for 20 minutes and the temperature was raised to 100° C. at a rate of 5° C. / min at the same time. Then, the mixture was switched to low-speed mixing at 180 rpm and fillers, flame retardants and lubricants were added in sequence. The mixture was mixed at low speed for 240 seconds to obtain a second mixture. After the second mixture was cooled, it was put into a twin-screw extruder for melt kneading and extrusion. The mixture was extruded and cooled to prepare pellets to obtain a cable material.
[0131] The mass ratio of polyvinyl chloride, stabilizer, filler, flame retardant, lubricant and plasticizer is 120:10:50:35:2:40. In addition, the stabilizer is calcium zinc stabilizer, the plasticizer is tricresol phosphate, the flame retardant is a mixture of aluminum hydroxide, hydrotalcite and montmorillonite in a mass ratio of 40:40:10, and the lubricant is polyethylene wax with a melting point of 115°C to 120°C.
[0132] The filler is prepared in the following manner:
[0133] Purified terephthalic acid and ethylene glycol were mixed and antimony trioxide was added as a catalyst to carry out esterification reaction. The reaction temperature was 250°C. When the water output of the esterification reaction reached 90% of the theoretical water output, the esterification reaction was stopped. After the esterification was completed, an organosilicon reagent was added to carry out polycondensation reaction. The reaction was first carried out at normal pressure for 0.5h, and then the vacuum was slowly evacuated to 100 Pa within 1.5h. The temperature of the whole system was then raised to 280°C and reacted for 1.5h to obtain a filler, wherein the organosilicon reagent includes the following structure:
[0134]
[0135] Example 5
[0136] This embodiment provides a flame-retardant cable material with high volume resistivity, and the preparation method thereof is as follows:
[0137] The polyvinyl chloride, stabilizer and plasticizer were stirred and mixed at 800 rpm for 20 minutes and the temperature was raised to 100° C. at a rate of 5° C. / min at the same time. Then, the mixture was switched to low-speed mixing at 180 rpm and fillers, flame retardants and lubricants were added in sequence. The mixture was mixed at low speed for 240 seconds to obtain a second mixture. After the second mixture was cooled, it was put into a twin-screw extruder for melt kneading and extrusion. The mixture was extruded and cooled to prepare pellets to obtain a cable material.
[0138] The mass ratio of polyvinyl chloride, stabilizer, filler, flame retardant, lubricant and plasticizer is 120:10:50:35:2:40. In addition, the stabilizer is calcium zinc stabilizer, the plasticizer is dioctyl phthalate, the flame retardant is aluminum hydroxide, and the lubricant is polyethylene wax with a melting point of 115°C to 120°C.
[0139] The filler is prepared in the following manner:
[0140] Purified terephthalic acid and ethylene glycol were mixed and antimony trioxide was added as a catalyst to carry out esterification reaction. The reaction temperature was 250°C. When the water output of the esterification reaction reached 90% of the theoretical water output, the esterification reaction was stopped. After the esterification was completed, an organosilicon reagent was added to carry out polycondensation reaction. The reaction was first carried out at normal pressure for 0.5h, and then the vacuum was slowly evacuated to 100 Pa within 1.5h. The temperature of the whole system was then raised to 280°C and reacted for 1.5h to obtain a filler, wherein the organosilicon reagent includes the following structure:
[0141]
[0142] Comparative Example 1
[0143] Compared with Example 1, most of the steps are the same except that no filler is added.
[0144] Comparative Example 2
[0145] Compared with Example 1, most of them are the same, except that the filler is changed to calcium carbonate.
[0146] Comparative Example 3
[0147] Compared with Example 1, most of the steps are the same, except that the organosilicon reagent in the filler is changed to 4-furandicarboxylic acid vinyl ester.
[0148] Test Case
[0149] 1. Tensile strength and elongation at break: The materials prepared in the examples and comparative examples were measured according to the method of GB / T2951-2008;
[0150] 2. Thermal oxygen aging resistance: The materials prepared in the examples and comparative examples were placed in an aging box and treated in an air atmosphere at 180°C for 168 hours, and the test was performed according to the method of GB / T 2951-2008;
[0151] 3. Oxygen index performance: Tested in accordance with GB / T 2406 standard.
[0152] The measurement results are shown in Table 1:
[0153]
[0154] From Example 1 to Example 5 and Comparative Examples 1 to Comparative Examples 3, the cable materials prepared in the present application have obvious improvements in mechanical properties such as tensile strength and elongation at break.
[0155] From Example 1 to Example 5, and Comparative Example 1 to Comparative Example 3, Example 5 simply adds flame retardant aluminum hydroxide, and its mechanical properties are reduced compared with Examples 1 to 4. This is because the simple flame retardant has poor compatibility with other components in the cable material, resulting in uneven distribution of the flame retardant, which increases the internal defects of the cable and causes the mechanical properties to decrease. In Examples 1 to 4, montmorillonite is present, which can improve compatibility, improve interfacial bonding, and effectively transfer stress through interfacial bonding, so that the mechanical properties are improved. When no filler is added in Comparative Example 1, and when the filler is changed to an inorganic filler in Comparative Example 2, the mechanical properties of the cable material decrease significantly, mainly because the filler provided in this application is a polar polymer, whose active group interacts with the tube energy group on the flame retardant, and its molecular chain can be combined with the flame retardant through physical entanglement and van der Waals force, thereby improving the interfacial adhesion between the components of the cable material. Although Comparative Example 3 is not an inorganic filler, it is not a polar polymer, and the interfacial bonding adhesion is limited, so that the mechanical properties of the cable material are not improved.
[0156] The oxygen index in Example 5 decreased significantly, mainly because the simple flame retardant aluminum hydroxide overheated due to internal friction during the extrusion plasticization process, resulting in decomposition and pores on the extruded cross section.
[0157] The oxygen index in Comparative Examples 1 to 3 decreased significantly, which is also because the flame retardant did not produce a synergistic effect with the filler. As mentioned above, the interface bonding force and compatibility were poor, which increased the internal defects of the cable and caused pores.
[0158] 4. Volume resistivity and contact angle test
[0159] First, the contact angles of the fillers in Examples 1 and 2 were tested. The contact angle of the filler in Example 1 was 134°, and the contact angle of the filler in Example 2 was 141°. Obviously, the hydrophobic properties of the filler can be precisely controlled by adjusting the side chain length, thereby increasing the water-blocking properties of the cable material, thereby making the volume resistivity of the cable material excellent.
[0160] In this application, the ion sources of polyvinyl chloride include the following aspects:
[0161] The first is the ions produced by chemical reactions of various compounding agents added to polyvinyl chloride, the second is the ions produced by the degradation of polyvinyl chloride itself, and the third is the dust and impurities in the production of polyvinyl chloride.
[0162] The volume resistivity was tested using GB / T8815-2008, and the test results are shown in Table 2:
[0163]
[0164] As shown in Table 1, among the embodiments of the present application, except for Example 5, the volume resistivity of the cable material is one order of magnitude higher than that of the comparative cable material. This is because the interaction between the filler used in the present application and the polyvinyl chloride macromolecular chain is weakened, and its active group interacts with the upper tube energy group in the flame retardant. Its molecular chain can be combined with the flame retardant through physical entanglement and van der Waals force to make its structure compact, so that the intermolecular force between polyvinyl chloride and the filler is weakened, thereby increasing the activation energy of ion migration, reducing the ion activity, and improving the volume resistivity. In Example 5, since the flame retardant does not contain montmorillonite, the filler used in the present application cannot synergize with the flame retardant, so that the interaction between the filler used in the present application and the polyvinyl chloride macromolecular chain is enhanced, resulting in a decrease in volume resistivity. After long-term immersion in water, it is found that the volume resistivity of the present application decreases by at least one order of magnitude. This is mainly because the hydrophobicity of the filler is strong, which increases the water-blocking property of the cable material, thereby causing the volume resistivity of the cable material to decrease less.
[0165] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A flame-retardant cable material with high volume resistivity, characterized in that: It includes the following components by weight: The filler is prepared in the following manner: The mixed purified terephthalic acid and ethylene glycol are subjected to esterification reaction, and after the esterification is completed, an organosilicon reagent is added to carry out polycondensation reaction to obtain a filler.
2. A flame-retardant cable material with high volume resistivity according to claim 1, characterized in that: The flame retardant cable material comprises the following components by weight:
3. A flame-retardant cable material with high volume resistivity according to claim 1 or 2, characterized in that: The esterification reaction and polycondensation reaction are carried out in a reactor; and / or, the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent is 1:(1-1.5):(1-1.5); And / or, the organosilicon reagent at least includes the compound described in the following formula (1): In the formula, R is a C0-C20 saturated alkyl group, R1 and R2 are the same or different and are each independently selected from phenyl or C1-C10 straight chain alkyl, X is selected from O or NH, m is a positive integer; And / or, the esterification reaction further requires the addition of a catalyst, the catalyst is preferably antimony trioxide, and the addition amount of antimony trioxide is 400-600 ppm; And / or, the reaction temperature of the esterification reaction is 240-260°C; and / or, when the water output of the esterification reaction reaches 90% of the theoretical water output, stopping the esterification reaction; And / or, after adding the organosilicon reagent, react at normal pressure for 0.5 to 1 hour, and then perform a pre-condensation treatment. The specific reaction conditions of the pre-condensation reaction are: slowly evacuate to 80 to 100 Pa within 1 to 3 hours, then raise the temperature of the entire system to 270 to 300° C., and react for 1 to 3 hours.
4. A flame-retardant cable material with high volume resistivity according to claim 1 or 2, characterized in that: The stabilizer is a mixture of one or more of lead stearate, barium stearate, barium laurate, zinc stearate, tribasic lead sulfate, dibasic lead phosphite, dibasic lead phthalate, lead silicate, lead cyanurate, and calcium stearate; And / or, the flame retardant is one or more combinations of antimony trioxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, and montmorillonite; And / or, the lubricant is one or more combinations of liquid paraffin, natural paraffin, microcrystalline paraffin, polyethylene wax, and stearic acid; And / or, the plasticizer is one or more combinations of dioctyl phthalate, tricresyl phosphate, diisononyl phthalate, dioctyl terephthalate, and trioctyl terephthalate.
5. A method for preparing a flame-retardant cable material with high volume resistivity, characterized in that: The steps include: The polyvinyl chloride, stabilizer and plasticizer are mixed by high-speed stirring, and the first mixture is obtained after heating. Then, the mixture is switched to low-speed mixing and fillers, flame retardants and lubricants are added in sequence to obtain a second mixture. After the second mixture is cooled, it is put into a twin-screw extruder for melt kneading and extrusion, extrusion cooling, and pellets are obtained to obtain a cable material.
6. The method for preparing a flame-retardant cable material with high volume resistivity according to claim 5, characterized in that: The high-speed stirring and mixing rate is 700-1000 rpm, and the high-speed stirring time is 20-60 min; And / or, the heating specifically comprises the following steps: heating to 90-100° C. at a rate of 5-8° C. / min; And / or, the low-speed mixing rate is 150 rpm-200 rpm, and the low-speed mixing time is 200-300 s; And / or, the cable material comprises the following components in parts by weight: 100-150 parts of polyvinyl chloride, 5-15 parts of stabilizer, 20-50 parts of filler, 20-40 parts of flame retardant, 1-3 parts of lubricant, and 30-50 parts of plasticizer.
7. The method for preparing a flame-retardant cable material with high volume resistivity according to claim 5, characterized in that: The filler is prepared in the following manner: The mixed purified terephthalic acid and ethylene glycol are subjected to esterification reaction, and after the esterification is completed, an organosilicon reagent is added to carry out polycondensation reaction to obtain a filler.
8. The method for preparing a flame-retardant cable material with high volume resistivity according to claim 7, characterized in that: The esterification reaction and polycondensation reaction are carried out in a reactor; and / or, the molar ratio of the purified terephthalic acid, ethylene glycol and the organosilicon reagent is 1:(1-1.5):(1-1.5); And / or, the organosilicon reagent at least includes the compound described in the following formula (1): In the formula, R is a C0-C20 saturated alkyl group, R1 and R2 are the same or different and are each independently selected from phenyl or C1-C10 straight chain alkyl, X is selected from O or NH, m is a positive integer; And / or, the esterification reaction further requires the addition of a catalyst, the catalyst is preferably antimony trioxide, and the addition amount of antimony trioxide is 400-600 ppm; And / or, the reaction temperature of the esterification reaction is 240-260°C; and / or, when the water output of the esterification reaction reaches 90% of the theoretical water output, stopping the esterification reaction; And / or, after adding the organosilicon reagent, react at normal pressure for 0.5 to 1 hour, and then perform a pre-condensation treatment. The specific reaction conditions of the pre-condensation reaction are: slowly evacuate to 80 to 100 Pa within 1 to 3 hours, then raise the temperature of the entire system to 270 to 300° C., and react for 1 to 3 hours.
9. The method for preparing a flame-retardant cable material with high volume resistivity according to claim 5, characterized in that: The stabilizer is a mixture of one or more of lead stearate, barium stearate, barium laurate, zinc stearate, tribasic lead sulfate, dibasic lead phosphite, dibasic lead phthalate, lead silicate, lead cyanurate, and calcium stearate; And / or, the flame retardant is one or more combinations of antimony trioxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, and montmorillonite; And / or, the lubricant is one or more combinations of liquid paraffin, natural paraffin, microcrystalline paraffin, polyethylene wax, and stearic acid; And / or, the plasticizer is one or more combinations of dioctyl phthalate, tricresyl phosphate, diisononyl phthalate, dioctyl terephthalate, and trioctyl terephthalate.
10. A cable material obtained by the method for preparing a flame-retardant cable material with high volume resistivity as claimed in any one of claims 5 to 9.
Citation Information
Patent Citations
Preparation method of flame-retardant anti-static cable material
CN108517089A
British standard PVC modified material and preparation method thereof
CN108841098A
Easily-dyed polyester DTY fiber and preparation method thereof
CN109735932A
Hydrolysis-resistant flame-retardant polyester and preparation method thereof
CN112724385A
Halogen-free flame-retardant anti-dripping PET copolyester and preparation method thereof
CN117510815A