Alcohol-resistant and heat-resistant PMMA composite material and preparation method thereof

By using polybutyl acrylate, modified dendrimer and nanoparticles in PMMA, an organic-inorganic dispersion system is formed, which solves the problem of insufficient heat and alcohol resistance of PMMA materials, and achieves high Transparency and excellent heat resistance.

CN118909379AInactive Publication Date: 2024-11-08CHENGDU ZHENCAI PLASTIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135568.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

PMMA materials have low heat resistance and are intolerant to alcohol, resulting in poor performance in high temperature and alcohol environments. Too much inorganic filler will reduce transparency, and too little will not meet the heat resistance requirements.

Method used

The enhancement additive is prepared by melt granulation of polybutyl acrylate, modified dendrimers and nanoparticles. Through hyperbranching and end group modification reactions, a dendrimer and epoxy silane coupling agent are formed to form an organic- The inorganic dispersion system combines the fluidity and compatibility of polybutyl acrylate to achieve improved heat and alcohol resistance of PMMA composites.

Benefits of technology

The heat resistance and alcohol tolerance of PMMA composite materials are significantly improved, ensuring uniformity of dispersion of inorganic particles and overall performance uniformity, while maintaining high transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999316880000081
    Figure BDA0004999316880000081
  • Figure BDA0004999316880000091
    Figure BDA0004999316880000091
Patent Text Reader

Abstract

The invention relates to an alcohol-resistant and heat-resistant PMMA (polymethyl methacrylate) composite material and a preparation method thereof, and belongs to the technical field of composite material preparation. The composite material is prepared from the following raw materials in parts by weight: 75 to 85 parts of PMMA (Polymethyl Methacrylate) base material, 15 to 25 parts of reinforcing aid, 0.1 to 1.3 parts of antioxidant and 0.1 to 1.3 parts of processing aid, the reinforcing auxiliary agent is prepared from poly (butyl acrylate), a modified dendrimer and nano-particles through melting granulation; the modified dendritic polymer is prepared by carrying out end group modification reaction on a dendritic polymer and an epoxy silane coupling agent, wherein the dendritic polymer is generated by carrying out hyperbranched reaction on silicon-chain-containing dihydric alcohol and tribasic acid. According to the invention, the heat resistance of PMMA and the tolerance of alcohol are improved at the same time through the introduction of the reinforcing auxiliary agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material preparation, and in particular relates to an alcohol-resistant and heat-resistant PMMA composite material and a preparation method thereof. Background Art

[0002] Polymethyl methacrylate (PMMA), with its unique advantages of light weight, easy molding and high transparency, is often widely used as an optical material. However, PMMA itself has low heat resistance, and inorganic fillers or high temperature resistant blended polymer materials are usually added to the PMMA base material to improve the heat resistance of its composite material. Among them, the addition of inorganic fillers is a commonly used heat-resistant enhancement method. In this heat-resistant enhancement method, the inorganic filler needs to be organically modified, which not only improves the heat resistance of the composite material, but also enhances the hardness and strength of the composite material. Too much inorganic filler addition will cause the PMMA composite material to reduce its transparency, and too little inorganic filler addition will not make the PMMA composite material meet the requirements of heat resistance. At the same time, PMMA has poor tolerance to alcohol, and the stains on its surface can only be cleaned with clean water, which makes it difficult to clean the surface of the PMMA board. Summary of the invention

[0003] The invention aims to provide an alcohol-resistant and heat-resistant PMMA composite material and a preparation method thereof.

[0004] The technical problem to be solved by the present invention is to improve the heat resistance and alcohol tolerance of PMMA.

[0005] One object of the present invention can be achieved by the following technical solutions:

[0006] An alcohol-resistant and heat-resistant PMMA composite material comprises the following raw materials in parts by weight: 75-85 parts of a PMMA base material, 15-25 parts of a reinforcing agent, 0.1-1.3 parts of an antioxidant, and 0.1-1.3 parts of a processing aid;

[0007] The reinforcing auxiliary agent is prepared by melt granulation of polybutyl acrylate, modified dendritic polymer and nanoparticles;

[0008] The modified dendrimer is prepared by a dendrimer generated by a hyperbranching reaction of a silicon-containing diol and a tribasic acid and an end group modification reaction of an epoxy silane coupling agent.

[0009] Furthermore, the mass ratio of the polybutyl acrylate, the modified dendritic polymer, and the nanoparticles is 8-16:15-30:15-30.

[0010] Furthermore, the silicon-chain diol is prepared by mixing 1,1,3,3-tetramethyldisiloxane and 2-propylene-1-ol in a molar ratio of 1:2.1-2.2 and subjecting the mixture to a hydrosilylation reaction.

[0011] Furthermore, the hydrosilylation reaction occurs in the presence of a platinum catalyst and an addition organic solvent, and the conditions of the hydrosilylation reaction are: a reaction temperature of 60-100° C. and a reaction time of 6-24 h.

[0012] Furthermore, the addition organic solvent is one of tetrahydrofuran, toluene and benzene.

[0013] Preferably, the preparation of the silicon-containing chain diol comprises the following steps:

[0014] After mixing 2-propylene-1-ol, an addition organic solvent and a platinum catalyst, the mixture is heated to the hydrosilylation reaction temperature, and then 1,1,3,3-tetramethyldisiloxane is added. After the addition is complete, the reaction is continued with stirring. After the reaction is completed, the mixture is cooled, filtered to recover the platinum catalyst, and the filtrate is rotated to recover the addition organic solvent to obtain a silicon-chain diol.

[0015] Furthermore, in the hyperbranching reaction, the molar ratio of the silicon-chain diol to the tribasic acid is 3.1-3.4:2, the hyperbranching reaction occurs in the presence of an esterification catalyst and an esterification organic solvent, and the conditions of the hyperbranching reaction are: the reaction temperature is 60-90°C and the reaction time is 4-6h.

[0016] Furthermore, the tribasic acid is citric acid.

[0017] Furthermore, the esterification catalyst is one of concentrated sulfuric acid (mass fraction is 98%), p-toluenesulfonic acid, thionyl chloride, phosphoric acid, boric acid, and sulfonic acid.

[0018] Furthermore, the esterification organic solvent is one of ethanol, ether, acetic acid, tetrahydrofuran, toluene, benzene, and dimethyl sulfate.

[0019] Preferably, the hyperbranching reaction comprises the following steps:

[0020] After mixing silicon-chain diol, tribasic acid and esterification organic solvent, add esterification catalyst dropwise, heat to hyperbranching reaction temperature, and stir to react at the same temperature. After the reaction is completed, recover the esterification organic solvent by rotary evaporation, wash with water, and dry to obtain dendrimer.

[0021] Furthermore, the end group modification reaction occurs under alkaline conditions and in the presence of a ring-opening organic solvent, and the conditions of the end group modification reaction are: reaction temperature of 55-85° C. and reaction time of 2-5 h.

[0022] Furthermore, the alkaline condition has a pH value of 9-10.

[0023] Furthermore, the ring-opening organic solvent is one of tetrahydrofuran, N,N-dimethylacetamide, toluene and benzene.

[0024] Furthermore, the mass ratio of the dendrimer to the epoxy silane coupling agent is 10:1-2.

[0025] Preferably, the end group modification reaction comprises the following steps:

[0026] After the dendrimer, epoxy silane coupling agent and ring-opening organic solvent are mixed, the pH value of the reaction system is adjusted to alkaline with sodium hydroxide solution, heated to the end group modification reaction temperature, and kept warm for reaction. After the reaction is completed, rotary evaporation, water washing and drying are performed to obtain the modified dendrimer.

[0027] Furthermore, the particle size of the nanoparticles is 100-200 nm; the nanoparticles are one or a mixture of nano carbon dioxide, nano calcium carbonate, nano magnesium hydroxide, and nano aluminum hydroxide.

[0028] Furthermore, the preparation of the reinforcing agent includes:

[0029] After the modified dendritic polymer and the nanoparticles are uniformly mixed, polybutyl acrylate is added, and the mixture is stirred and mixed at 80-100° C. for 10-15 minutes to obtain a mixture; the mixture is melt-extruded and granulated at 150-190° C. by a twin-screw extruder to obtain a reinforcing auxiliary agent.

[0030] Another object of the present invention can be achieved by the following technical solutions:

[0031] A method for preparing an alcohol-resistant and heat-resistant PMMA composite material, characterized in that:

[0032] The PMMA base material, reinforcing auxiliary agent, antioxidant and processing auxiliary agent are melt-extruded and granulated through a twin-screw extruder to obtain a composite material, wherein the extrusion temperature is 200-240°C.

[0033] Beneficial effects of the present invention:

[0034] The present invention improves the heat resistance and alcohol tolerance of PMMA by introducing a reinforcing auxiliary agent. The reinforcing auxiliary agent is a master batch prepared by melt extrusion, and the master batch uses polybutyl acrylate and a modified dendritic polymer as the loading resin, and utilizes the excellent fluidity of polybutyl acrylate and its excellent compatibility with PMMA, and the loading property of the modified dendritic polymer. First, the modified dendritic polymer and nanoparticles are mixed, and the nanoparticles are loaded and modified by using the siloxane at the end of the modified dendritic polymer to form an organic-inorganic preliminary mixed dispersion system, and then the excellent fluidity of polybutyl acrylate is utilized to load the organic-inorganic dispersion system with the polybutyl acrylate organic chain (butyl alkyl chain and the silicon cation in the dendritic molecule) The backbone chain or siloxane chain is entangled, thereby realizing the loading of the organic-inorganic dispersion system), forming an organic-inorganic final dispersion system, in which not only the inorganic nanoparticles are evenly dispersed, but also the main chain (long chain) of polybutyl acrylate is possessed, and the long chain is the same as the main chain of PMMA, and acts as a compatibilizer between PMMA and the organic-inorganic final dispersion system, thereby realizing the excellent dispersion uniformity of the organic-inorganic final dispersion system in PMMA, and this uniformity not only ensures the dispersion uniformity of the inorganic particles, but also ensures the dispersion uniformity of the dendrimer polymer, so that the overall performance of the obtained composite material is uniform;

[0035] Significantly, the dendrimer molecules contain a large number of silicon-cationic bonds (derived from 1,1,3,3-tetramethyldisiloxane), which have high silicon-cationic bond energy and good heat resistance, and their introduction improves the heat resistance of the obtained composite material; at the same time, nano carbon dioxide, nano calcium carbonate, nano magnesium hydroxide, and nano aluminum hydroxide are all heat-resistant inorganic nanoparticles, which together with the dendrimer improve the heat resistance of the obtained composite material;

[0036] Finally, the siloxane chains at the ends of the dendrimers endow the resulting composites with excellent alcohol resistance. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] Preparation of modified dendrimers

[0040] i. After mixing 0.21 mol 2-propylene-1-ol, 100 mL tetrahydrofuran and a platinum catalyst, the mixture is heated to 65°C, followed by adding 0.1 mol 1,1,3,3-tetramethyldisiloxane. After the addition is complete, the mixture is stirred and reacted for 6 hours. After the reaction is completed, the mixture is cooled, filtered and the platinum catalyst is recovered, and the filtrate is rotary evaporated to recover tetrahydrofuran to obtain a silicon-containing chain diol, wherein the platinum catalyst is a platinum-supported catalyst, such as Pt / C, with a loading mass fraction of 5%, and the mass of Pt added is 3% of the mass of the raw material;

[0041] ii. After mixing 0.31 mol of silicon-containing diol (based on the molar mass of 1,1,3,3-tetramethyldisiloxane), 0.2 mol of citric acid and 100 mL of ethanol, concentrated sulfuric acid was added dropwise, heated to reflux, and stirred under reflux for 4 hours. After the reaction was completed, the solvent was recovered by rotary evaporation, washed with water, and dried to obtain a dendrimer, wherein the mass of concentrated sulfuric acid added was 2% of the mass of the raw material;

[0042] iii. After mixing 60 g of dendrimer, 6 g of epoxy silane coupling agent (KH560) and 100 mL of tetrahydrofuran, the pH value of the reaction system was adjusted to 9-10 with sodium hydroxide solution, heated to 55 ° C, and kept warm for 5 hours. After the reaction was completed, rotary evaporation, water washing, and drying were performed to obtain a modified dendrimer.

[0043] Example 2

[0044] Preparation of modified dendrimers

[0045] i. After mixing 0.22 mol 2-propylene-1-ol, 100 mL tetrahydrofuran and an excess of platinum catalyst, the mixture is heated to 65°C, followed by adding 0.1 mol 1,1,3,3-tetramethyldisiloxane. After the addition is complete, the mixture is stirred and reacted for 24 hours. After the reaction is completed, the mixture is cooled, filtered and the platinum catalyst is recovered, and the filtrate is evaporated and the organic solvent is recovered to obtain a silicon-containing diol, wherein the platinum catalyst is a platinum-supported catalyst, such as Pt / C, and the loading mass fraction is 5%, and the mass of Pt added is 3% of the mass of the raw material;

[0046] ii. After mixing 0.34 mol of silicon-containing diol (based on the molar mass of 1,1,3,3-tetramethyldisiloxane), 0.2 mol of citric acid and 120 mL of ethanol, concentrated sulfuric acid was added dropwise, heated to reflux, and refluxed with stirring for 6 hours. After the reaction was completed, the solvent was evaporated back, washed with water, and dried to obtain a dendrimer, wherein the mass of concentrated sulfuric acid added was 2% of the mass of the raw material;

[0047] iii. After mixing 60 g of dendrimer, 12 g of epoxy silane coupling agent (KH560) and 100 mL of tetrahydrofuran, the pH value of the reaction system was adjusted to 9-10 with sodium hydroxide solution, heated to 60 ° C, and kept warm for 2 hours. After the reaction was completed, rotary evaporation, water washing, and drying were performed to obtain a modified dendrimer.

[0048] Example 3

[0049] Preparation of reinforcing additives:

[0050] S1. After 15 g of the modified dendritic polymer prepared in Example 1 and 30 g of the nanoparticles are uniformly mixed, 16 g of polybutyl acrylate is added, and the mixture is stirred at 80° C. for 15 min to obtain a mixture;

[0051] S2. The mixed material is melt-extruded and granulated at 150-190° C. through a twin-screw extruder to obtain a reinforcing auxiliary agent.

[0052] Example 4

[0053] Preparation of reinforcing additives:

[0054] S1. After 30 g of the modified dendritic polymer prepared in Example 2 and 15 g of nanoparticles are uniformly mixed, 8 g of polybutyl acrylate is added, and the mixture is stirred and mixed at 100° C. for 10 min to obtain a mixture;

[0055] S2. The mixed material is melt-extruded and granulated at 150-190° C. through a twin-screw extruder to obtain a reinforcing auxiliary agent.

[0056] Example 5

[0057] Preparation of composite materials:

[0058] C1. Prepare the following raw materials in parts by weight: 75 parts of PMMA base material, 25 parts of reinforcing agent, 0.1 parts of antioxidant, and 0.1 parts of processing aid;

[0059] The antioxidant is antioxidant 1010, the processing auxiliary component is a lubricant, and the lubricant is polyethylene wax;

[0060] C2. The PMMA base material, reinforcing agent, antioxidant and processing aid are melt-extruded and granulated through a twin-screw extruder to obtain a composite material, wherein the extrusion temperature is 200-240°C.

[0061] Example 6

[0062] Preparation of composite materials:

[0063] C1. Prepare the following raw materials in parts by weight: 80 parts of PMMA base material, 20 parts of reinforcing agent, 1 part of antioxidant, and 1 part of processing aid;

[0064] The antioxidant is antioxidant 1010, the processing auxiliary component is a lubricant, and the lubricant is polyethylene wax;

[0065] C2. The PMMA base material, reinforcing agent, antioxidant and processing aid are melt-extruded and granulated through a twin-screw extruder to obtain a composite material, wherein the extrusion temperature is 200-240°C.

[0066] Example 7

[0067] Preparation of composite materials:

[0068] C1. Prepare the following raw materials in parts by weight: 85 parts of PMMA base material, 15 parts of reinforcing agent, 1.3 parts of antioxidant, and 1.3 parts of processing aid;

[0069] The antioxidant is antioxidant 1010, the processing auxiliary component is a lubricant, and the lubricant is polyethylene wax;

[0070] C2. The PMMA base material, reinforcing agent, antioxidant and processing aid are melt-extruded and granulated through a twin-screw extruder to obtain a composite material, wherein the extrusion temperature is 200-240°C.

[0071] Comparative Example 1

[0072] Preparation of reinforcing aid: Compared with Example 3, an equal amount of the modified dendritic polymer was replaced with the dendritic polymer prepared in step ii of Example 1, and the rest was the same.

[0073] Comparative Example 2

[0074] Preparation of reinforcing auxiliary agent: Compared with Example 3, the modified dendritic polymer was deleted, and the rest was the same.

[0075] Comparative Example 3

[0076] Preparation of reinforcing auxiliary agent: Compared with Example 3, polybutyl acrylate was deleted, and the rest was the same.

[0077] Comparative Example 4

[0078] Preparation of composite materials: Compared with Example 5, an equal amount of the reinforcing aid is replaced with the reinforcing aid prepared in Comparative Example 1, and the rest is the same.

[0079] Comparative Example 5

[0080] Preparation of composite materials: Compared with Example 5, an equal amount of the reinforcing aid is replaced with the reinforcing aid prepared in Comparative Example 2, and the rest is the same.

[0081] Comparative Example 6

[0082] Preparation of composite materials: Compared with Example 5, an equal amount of the reinforcing aid is replaced with the reinforcing aid prepared in Comparative Example 3, and the rest is the same.

[0083] Comparative Example 7

[0084] Preparation of composite material: Compared with Example 5, the reinforcing auxiliary agent was deleted, and the rest was the same.

[0085] The PMMA base materials in the above embodiments are all Acrypet IR H50 from Mitsubishi, Japan.

[0086] The composite materials obtained in Examples 5-7 and Comparative Examples 4-7 were subjected to performance tests, and the results of the performance tests are shown in Table 1. The transmittance of the composite material molded sheet was measured using a UV-3600p l us ultraviolet visible near infrared spectrophotometer produced by Shimadzu Corporation of Japan; alcohol resistance: according to GB / T 11547, the composite material was immersed in 79% ethanol by volume for 24 hours, taken out, dried, and the transmittance was measured, and the decrease rate of the transmittance was calculated; the heat deformation temperature was tested according to ISO 75-2; the scratch resistance was tested according to the pencil method in GB / T 6739 (the scratch resistance levels were arranged in descending order as 6H, 5H, 4H, 3H, 2H, H, HB);

[0087] Table 1

[0088]

[0089]

[0090] It can be seen from Table 1 that the composite materials obtained in Examples 5-7 of the present invention have excellent transparency, alcohol resistance and heat resistance.

[0091] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0092] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An alcohol-resistant and heat-resistant PMMA composite material, characterized in that: The raw materials include the following parts by weight: 75-85 parts of PMMA base material, 15-25 parts of reinforcing agent, 0.1-1.3 parts of antioxidant, and 0.1-1.3 parts of processing auxiliary agent; The reinforcing auxiliary agent is prepared by melt granulation of polybutyl acrylate, modified dendritic polymer and nanoparticles; The modified dendrimer is prepared by a dendrimer generated by a hyperbranching reaction of a silicon-containing diol and a tribasic acid and an end group modification reaction of an epoxy silane coupling agent.

2. The alcohol-resistant and heat-resistant PMMA composite material according to claim 1, characterized in that: The mass ratio of the polybutyl acrylate, the modified dendritic polymer and the nanoparticles is 8-16:15-30:15-30.

3. The alcohol-resistant and heat-resistant PMMA composite material according to claim 1, characterized in that: The silicon-chain-containing diol is prepared by mixing 1,1,3,3-tetramethyldisiloxane and 2-propylene-1-ol in a molar ratio of 1:2.1-2.2 and undergoing a hydrosilylation reaction.

4. The alcohol-resistant and heat-resistant PMMA composite material according to claim 3, characterized in that: The hydrosilylation reaction occurs in the presence of a platinum catalyst and an addition organic solvent, and the conditions of the hydrosilylation reaction are: a reaction temperature of 60-100° C. and a reaction time of 6-24 hours.

5. The alcohol-resistant and heat-resistant PMMA composite material according to claim 4, characterized in that: The addition organic solvent is one of tetrahydrofuran, toluene and benzene.

6. The alcohol-resistant and heat-resistant PMMA composite material according to claim 1, characterized in that: In the hyperbranching reaction, the molar ratio of silicon-chain diol to tribasic acid is 3.1-3.4:

2. The hyperbranching reaction occurs in the presence of an esterification catalyst and an esterification organic solvent. The conditions of the hyperbranching reaction are: reaction temperature of 60-90°C, reaction time of 4-6h; and the tribasic acid is citric acid.

7. The alcohol-resistant and heat-resistant PMMA composite material according to claim 1, characterized in that: The end group modification reaction occurs under alkaline conditions and in the presence of a ring-opening organic solvent. The conditions of the end group modification reaction are: a reaction temperature of 55-85° C. and a reaction time of 2-5 hours.

8. The alcohol-resistant and heat-resistant PMMA composite material according to claim 1, characterized in that: The particle size of the nanoparticles is 100-200nm; the nanoparticles are one or a mixture of nano carbon dioxide, nano calcium carbonate, nano magnesium hydroxide and nano aluminum hydroxide.

9. The alcohol-resistant and heat-resistant PMMA composite material according to claim 1, characterized in that: The preparation of the reinforcing aid comprises: After the modified dendritic polymer and the nanoparticles are uniformly mixed, polybutyl acrylate is added, and the mixture is stirred at 80-100° C. for 10-15 minutes to obtain a mixture; The mixed material is melt-extruded and granulated at 150-190° C. through a twin-screw extruder to obtain a reinforcing auxiliary agent.

10. The method for preparing an alcohol-resistant and heat-resistant PMMA composite material according to any one of claims 1 to 9, characterized in that: include: The PMMA base material, reinforcing auxiliary agent, antioxidant and processing auxiliary agent are melt-extruded and granulated through a twin-screw extruder to obtain a composite material.