Preparation method and application of special toughening impact modifier for PP (polypropylene)

By grafting and modifying on the polyolefin elastomer and adding specific ethylene copolymers, a new PP-specific toughening impact modifier was prepared, which solved the problem of insufficient impact performance of polypropylene materials, and achieved the rigidity of polypropylene materials and Toughness balance improves application and processing stability.

CN118909386AInactive Publication Date: 2024-11-08BOXUN CHEMICAL TECHNOLOGY (HENAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411107607.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The impact performance of polypropylene materials is insufficient. The existing toughening modifiers are prone to lose mechanical properties, especially strength, when improving impact toughness, and have an impact on injection molding process and product quality.

Method used

By grafting modification on the polyolefin elastomer, adding ethylene copolymer of a specific molecular weight and maleic anhydride to form the first graft and blending it with the ethylene copolymer, a new type of PP special toughening is prepared Impact modifiers regulate their dispersion and compatibility in polypropylene through coextrusion and blending techniques to achieve balance of toughening effects.

Benefits of technology

It significantly improves the rigidity and toughness balance of polypropylene materials, enhances its application, avoids the negative impact on mechanical properties, and improves processing stability and toughening effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991261620000061
    Figure BDA0004991261620000061
  • Figure BDA0004991261620000071
    Figure BDA0004991261620000071
Patent Text Reader

Abstract

The invention relates to the field of preparation of polymer auxiliaries, and particularly discloses a preparation method and application of a special toughening impact modifier for PP (polypropylene), and the preparation method comprises the following steps: (1) preparation of a first graft: adding a polyolefin elastomer, a first monomer, a second monomer and an initiator into a reactor, stirring and mixing, and continuously extruding to obtain the first graft; and (2) preparation of the toughening impact modifier: adding the first graft and the ethylene copolymer into a reactor, stirring and mixing, and carrying out melt blending, extrusion and granulation to obtain the toughening impact modifier. The toughening impact modifier disclosed by the invention has a remarkable effect when being used for toughening impact modification of a polypropylene material, realizes the balance between rigidity and toughness of the polypropylene material, and can effectively improve the applicability of the polypropylene material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer auxiliary preparation, and particularly relates to a preparation method and application of a special toughening and impact modifier for PP. Background Art

[0002] Polypropylene (PP) is a general-purpose resin with good heat resistance, corrosion resistance and mechanical properties. It has been widely used in various industries such as automotive industrial products, daily products, and biomedicine. However, the insufficient impact performance of polypropylene, that is, poor impact toughness, seriously restricts its application.

[0003] The toughening and modification methods for polypropylene mainly include chemical modification and physical modification. Chemical modification is to introduce toughening and modification groups into the polypropylene molecular chain segments to improve the impact toughness, but the chemical modification process is cumbersome; physical modification is to add modifiers for blending, which has a simple and flexible process and high practicality. In the prior art, EPDM rubber and ethylene-octene copolymer are often added as modifiers to modify polypropylene. However, the addition amount of the above modifiers is large, which can easily cause other properties of polypropylene materials, especially mechanical properties and strength losses.

[0004] The invention patent with application number 201210523848.3 discloses a polypropylene toughening modifier and a polypropylene modified product thereof. The composition and proportion of the polypropylene toughening modifier are as follows: polyethylene 15-50wt%, polypropylene 15-50wt%, ethylene and octene copolymer POE 20-55wt%, initiator 0.1-2.0wt%, antioxidant 0.05-1.0wt%. The impact strength of the polypropylene modified product obtained by physical blending with polypropylene and extrusion injection molding is increased by 28-34.5%, which effectively reduces the slow secondary crystallization phenomenon of the polypropylene modified product during the later storage process and greatly eliminates the residual internal stress of the polypropylene modified product. However, the toughening modifier may reduce the melt fluidity of polypropylene, which has a certain impact on the polypropylene injection molding process and product quality.

[0005] In view of this, it is particularly important to disclose a special toughening and impact modifier for PP in this application. Summary of the invention

[0006] In view of the defects of the prior art, the present invention discloses a preparation method and application of a special toughening and impact modifier for PP. The toughening and impact modifier disclosed in the present invention has a significant effect when used for toughening and impact modification of polypropylene materials, achieves a balance between the rigidity and toughness of polypropylene materials, and can effectively improve the applicability of polypropylene materials.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] The present invention provides a method for preparing a special toughening and impact modifier for PP, comprising the following steps:

[0009] (1) Preparation of the first grafted product: adding a polyolefin elastomer, a first monomer, a second monomer and an initiator into a reactor, stirring and mixing, and continuously extruding to obtain a first grafted product;

[0010] (2) Preparation of toughened impact modifier: The first grafted material and the ethylene copolymer are added into a reactor, stirred and mixed, melt blended, extruded and granulated to obtain the toughened impact modifier.

[0011] In some embodiments of the present invention, the polyolefin elastomer in step (1) is an ethylene / α-olefin random copolymer, and the melt flow rate measured at 230° C. with a load of 2.16 kg is (3 to 5) g / 10 min.

[0012] Preferably, the polyolefin elastomer in step (1) is ethylene-octene random copolymer.

[0013] Preferably, in the step (1), the melt flow rate of the polyolefin elastomer measured at 230° C. and a load of 2.16 kg is 4 g / 10 min.

[0014] In some embodiments of the present invention, the first monomer in step (1) is maleic anhydride.

[0015] In some embodiments of the present invention, the second monomer in step (1) is 2-hydroxyethyl acrylate.

[0016] In some embodiments of the present invention, the mass ratio of the polyolefin elastomer, the first monomer, and the second monomer in step (1) is 10:(1.1-1.6):(2-3).

[0017] Preferably, in step (1), the mass ratio of the polyolefin elastomer, the first monomer and the second monomer is 10:1.3:2.5.

[0018] In some embodiments of the present invention, the conditions for continuous extrusion in step (1) are: temperature 150-200° C., rotation speed 300-550 r / min.

[0019] In some embodiments of the present invention, the number average molecular weight of the ethylene copolymer in step (2) is ≥10,000.

[0020] Preferably, the number average molecular weight of the ethylene copolymer in step (2) is 10,000 to 90,000.

[0021] Preferably, the number average molecular weight of the ethylene copolymer in step (2) is 50,000.

[0022] In some embodiments of the present invention, the mass ratio of the first grafted substance to the ethylene copolymer in step (2) is 100:(0.2-1).

[0023] Preferably, in step (2), the mass ratio of the first grafted product to the ethylene copolymer is 100:0.6.

[0024] In some embodiments of the present invention, the melt blending in step (2) is carried out in a twin-screw extruder with a set temperature of 190 to 220° C. and a rotation speed of 200 to 450 r / min.

[0025] Another aspect of the present invention provides a use of a special toughening and impact modifier for PP obtained by the above preparation method in the preparation of PP, wherein the addition amount of the toughening and impact modifier is 3-8wt% of the PP.

[0026] Preferably, the toughening and impact modifier is added in an amount of 6.5 wt % of PP.

[0027] The present invention adds a first monomer and a second monomer to perform co-extrusion modification on a polyolefin elastomer with a specific melt flow rate, and the obtained first graft has a narrow relative molecular weight distribution and high branch symmetry, and has excellent toughening performance. When the first graft is added to a polypropylene material, it can achieve a dispersibility far exceeding that of other toughening modifiers, and the dispersion is more uniform. An excellent toughening effect can be achieved with a smaller addition amount. The possible reason is that due to the better dispersibility in the matrix, the toughening impact modifier containing the first graft chain segment is evenly and densely distributed in the "sea phase" polypropylene as an "island phase", and is stretched into microfibers when subjected to external force impact, which absorbs more impact energy on the one hand and prevents silver streaks from developing into cracks on the other hand, thereby achieving a better toughening effect.

[0028] The applicant found that although the polyolefin elastomer has better toughening performance after the above grafting modification, it may have an adverse effect on the rigidity of polypropylene when added to the polypropylene material system. In view of this, the applicant obtained a new toughening and impact modifier by introducing a specific molecular weight ethylene copolymer and adjusting the blending ratio of it and the first graft. When it modifies polypropylene, it can achieve efficient toughening effect while avoiding the influence on the mechanical properties of polypropylene materials, and achieves a balance between the rigidity and toughness of polypropylene materials. The possible reason is that the addition of the specific molecular weight ethylene copolymer inhibits the degradation of polypropylene caused by maleic anhydride monomer; on the other hand, when the ethylene copolymer and the first graft are blended, the maleic anhydride present in the side chain of the polyolefin elastomer changes the regularity of the polymer molecular chain. It may also be due to the similar olefin segments of the ethylene copolymer and the first graft, so that the two phases have extremely high compatibility, which improves the processing stability of the toughening and impact modifier; on the other hand, the specific molecular weight ethylene copolymer also plays a certain interweaving network role, which is conducive to further improving the toughening effect of the first elastomer on polypropylene.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The toughening and impact modifier disclosed in the present invention is effective in toughening and impact modifying polypropylene materials, achieving a balance between the rigidity and toughness of polypropylene materials, and can effectively improve the applicability of polypropylene materials.

[0031] (2) The present invention adds a first monomer and a second monomer to co-extrude a polyolefin elastomer with a specific melt flow rate to modify the obtained first grafted product, and the obtained first grafted product has a narrow relative molecular weight distribution and high branch symmetry, and has excellent toughening performance. When the first grafted product is added to polypropylene, it can achieve a dispersibility far exceeding that of other toughening modifiers, and the dispersion is more uniform, and an excellent toughening effect can be achieved at a relatively small addition amount.

[0032] (3) The present invention obtains a new type of toughening and impact modifier by introducing an ethylene copolymer with a specific molecular weight and adjusting the blending ratio between the ethylene copolymer and the first grafted product. When the ethylene copolymer is used to modify polypropylene, it can achieve a high-efficiency toughening effect while avoiding the influence on the mechanical properties of the polypropylene material, thereby achieving a balance between the rigidity and toughness of the polypropylene material.

[0033] (4) In the present invention, when the ethylene copolymer and the first grafted product are blended, the maleic anhydride present in the side chain of the polyolefin elastomer changes the regularity of the polymer molecular chain, increases the compatibility between the two phases, and improves the processing stability of the toughening and impact modifier; on the other hand, the ethylene copolymer with a specific molecular weight also plays a certain interweaving network role, which is beneficial to further improve the toughening effect of the first elastomer on polypropylene. DETAILED DESCRIPTION

[0034] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0035] Unless otherwise specified, the reagents used below can be easily obtained from commercial companies, wherein ethylene copolymers (number average molecular weight of 8000 and 50000) were purchased from Suzhou Daman Engineering Plastics Co., Ltd.

[0036] Unless otherwise specified, the melt flow rate (230°C / 2.16kg) of the ethylene-octene random copolymer used in the following examples and comparative examples is 4 g / 10 min.

[0037] Example 1

[0038] A method for preparing a special toughening and impact modifier for PP, comprising the following steps:

[0039] (1) Preparation of the first grafted product: 100 g of ethylene-octene random copolymer, 13 g of maleic anhydride, 25 g of 2-hydroxyethyl acrylate and 0.69 g of benzoyl peroxide were added to a reactor, stirred and mixed, and continuously extruded at a temperature of 175° C. and a rotation speed of 425 r / min to obtain a first grafted product;

[0040] (2) Preparation of toughened impact modifier: 100 g of the first grafted material and 0.6 g of ethylene copolymer were added to a reactor, stirred and mixed, and extruded and granulated in a twin-screw extruder at a temperature of 205° C. and a rotation speed of 325 r / min to obtain a toughened impact modifier.

[0041] Example 2

[0042] A method for preparing a special toughening and impact modifier for PP, comprising the following steps:

[0043] (1) Preparation of the first grafted product: 100 g of ethylene-octene random copolymer, 11 g of maleic anhydride, 20 g of 2-hydroxyethyl acrylate and 0.66 g of benzoyl peroxide were added to a reactor, stirred and mixed, and continuously extruded at a temperature of 150° C. and a rotation speed of 550 r / min to obtain a first grafted product;

[0044] (2) Preparation of toughened impact modifier: 100 g of the first grafted material and 1 g of ethylene copolymer were added to a reactor, stirred and mixed, and extruded and granulated in a twin-screw extruder at a set temperature of 190° C. and a rotation speed of 450 r / min to obtain a toughened impact modifier.

[0045] Example 3

[0046] A method for preparing a special toughening and impact modifier for PP, comprising the following steps:

[0047] (1) Preparation of the first grafted product: 100 g of ethylene-octene random copolymer, 16 g of maleic anhydride, 30 g of 2-hydroxyethyl acrylate and 0.73 g of benzoyl peroxide were added to a reactor, stirred and mixed, and continuously extruded at a temperature of 200° C. and a rotation speed of 300 r / min to obtain a first grafted product;

[0048] (2) Preparation of toughened impact modifier: 100 g of the first grafted material and 0.2 g of ethylene copolymer were added to a reactor, stirred and mixed, and extruded and granulated in a twin-screw extruder at a set temperature of 220° C. and a rotation speed of 200 r / min to obtain a toughened impact modifier.

[0049] Example 4

[0050] A method for preparing a special toughening and impact modifier for PP, the specific implementation method is the same as that of Example 1, except that the amount of maleic anhydride added in step (1) is 19g.

[0051] Example 5

[0052] A method for preparing a special toughening and impact modifier for PP, the specific implementation method is the same as that of Example 1, except that the amount of ethylene copolymer added in step (2) is 1.2 g.

[0053] Example 6

[0054] A method for preparing a special toughening and impact modifier for PP, the specific implementation method is the same as that of Example 1, except that the number average molecular weight of the ethylene copolymer in step (2) is 8000.

[0055] Comparative Example 1

[0056] A method for preparing a special toughening and impact modifier for PP, comprising the following steps:

[0057] 100 g of ethylene-octene random copolymer, 13 g of maleic anhydride, 25 g of 2-hydroxyethyl acrylate and 0.69 g of benzoyl peroxide were added into a reactor, stirred and mixed, and continuously extruded at a temperature of 200° C. and a rotation speed of 300 r / min to obtain a toughened impact modifier.

[0058] Comparative Example 2

[0059] A method for preparing a special toughening and impact modifier for PP, the specific implementation method is the same as that of Example 1, except that in step (1), 38g of maleic anhydride is used to replace 13g of maleic anhydride and 25g of 2-hydroxyethyl acrylate.

[0060] Performance Testing:

[0061] The toughening and impact modifier obtained in the above embodiments and comparative examples was mixed with polypropylene (6.5 g of toughening and impact modifier was added to every 100 g of polypropylene), melt-extruded and granulated at 200° C. by a twin-screw extruder, with a screw speed of 240 r / min. The pellets were then injection-molded by an injection molding machine at an injection molding temperature of 210° C., an injection molding pressure of 40 MPa, and a holding time of 15 s to obtain test samples, and performance tests were carried out under the same conditions as follows. The specific test results are shown in Table 1.

[0062] (1) Tensile property test: The test was carried out on a WDW3050 electronic universal testing machine of Changchun Kexin Experimental Instrument Co., Ltd. in accordance with standard GB / T1040.1-2006. The tensile speed was 50 mm / min and the test sample size was 75 mm × 4 mm × 1 mm.

[0063] (2) Bending property test: The test was carried out in accordance with the standard GB / T 9341-2008 on a WDW3050 electronic universal testing machine of Changchun Kexin Experimental Instrument Co., Ltd. The test speed was 2 mm / min, the span was 64 mm, and the test sample size was 80 mm × 10 mm × 4 mm;

[0064] (3) Impact resistance test: The test was carried out in accordance with standard GB / T1043.1-2008 on an XJJ-50 impact tester from Chengde Dahua Testing Machine Co., Ltd. The test sample size was 80 mm × 10 mm × 4 mm, with a V-notch and a notch depth of 2.54 mm. The impact rate was 3.5 m / s and the pendulum weight was 0.818 kg.

[0065] Table 1

[0066]

[0067]

[0068] As can be seen from Table 1, the PP-specific toughening and impact modifier disclosed in Examples 1 to 3 of the present invention has a significant effect when used for toughening and impact modification of polypropylene materials, and the tensile strength, flexural strength and impact strength of polypropylene are all significantly improved.

[0069] From the comparison between Example 4 and Example 1, it can be seen that when the grafting amount of maleic anhydride used to prepare the first grafted product is changed, the dispersion effect is affected, which will eventually lead to a decrease in the tensile strength, flexural strength and impact strength of the polypropylene material;

[0070] From the comparison between Example 5 and Example 1, it can be seen that when the mass ratio of the first grafted product to the ethylene copolymer is changed, the mitigation effect of the side effects of the maleic anhydride monomer is affected, which will lead to a decrease in the performance of the polypropylene material, especially the impact strength;

[0071] From the comparison between Example 6 and Example 1, it can be seen that when the molecular weight of the ethylene copolymer compounded with the first graft material changes, the processing performance of the polypropylene material will be reduced, and finally the tensile strength, flexural strength and impact strength of the finished product will decrease to varying degrees;

[0072] From the comparison between Comparative Example 1 and Example 1, it can be seen that when the ethylene copolymer is not added to the first graft compound, the degradation of polypropylene caused by the maleic anhydride monomer will cause the overall performance of the polypropylene material to decrease;

[0073] From the comparison between Comparative Example 2 and Example 1, it can be seen that modifying the polyolefin copolymer with only maleic anhydride monomer will lead to a decrease in the tensile strength, flexural strength and impact strength of the polypropylene material.

[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a special toughening and impact modifier for PP, characterized in that: The following steps are involved: (1) Preparation of the first grafted product: adding a polyolefin elastomer, a first monomer, a second monomer and an initiator into a reactor, stirring and mixing, and continuously extruding to obtain a first grafted product; (2) Preparation of toughened impact modifier: The first grafted material and the ethylene copolymer are added into a reactor, stirred and mixed, melt blended, extruded and granulated to obtain the toughened impact modifier.

2. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: The polyolefin elastomer in step (1) is an ethylene / α-olefin random copolymer, and the melt flow rate measured at 230° C. and 2.16 kg load is (3-5) g / 10 min.

3. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: In the step (1), the first monomer is maleic anhydride.

4. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: The second monomer in step (1) is 2-hydroxyethyl acrylate.

5. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: In the step (1), the mass ratio of the polyolefin elastomer, the first monomer and the second monomer is 10:(1.1-1.6):(2-3).

6. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: The conditions for continuous extrusion in step (1) are: temperature 150-200° C., rotation speed 300-550 r / min.

7. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: The number average molecular weight of the ethylene copolymer in the step (2) is ≥10,000.

8. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: In the step (2), the mass ratio of the first grafted product to the ethylene copolymer is 100:(0.2-1).

9. The method for preparing a special toughening and impact modifier for PP according to claim 1, characterized in that: The melt blending in step (2) is performed in a twin-screw extruder with a temperature set at 190 to 220° C. and a rotation speed set at 200 to 450 r / min.

10. Use of a special toughening and impact modifier for PP obtained by the preparation method according to any one of claims 1 to 9 in the preparation of PP, characterized in that: The amount of the toughening and impact modifier added is 3-8wt% of PP.