High-impact high-modulus polypropylene material as well as preparation method and application thereof

By adding bimodal polyethylene resin and phosphate additives to the polypropylene material, combining specific copolymerized polypropylene resin and crosslinking agent, the problem of difficulty in achieving high impact strength and high modulus in the prior art is solved, and the problem of achieving high impact strength and high modulus is achieved. Polypropylene material with high impact strength and good mechanical properties is suitable for communication junction boxes.

CN118909389APending Publication Date: 2024-11-08KUNSHAN SUNWILL ENG PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149239.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

It is difficult for existing communication junction box materials to achieve high impact strength and high modulus at the same time, resulting in the problems of deformation and airtight failure when used in harsh environments.

Method used

20%-30% first copolymer polypropylene resin, 20%-30% second copolymer polypropylene resin, 3%-8% bimodal polyethylene resin, 5%-10% compatibility agent, 0.2%-1.0% A combination of crosslinking agent, 25%-35% glass fiber, 0.1%-0.5% phosphate additives, adjust the acidity and alkalinity of the material through the unique molecular weight distribution of bimodal polyethylene resin and the phosphate additives, combining with specific copolymerization Polypropylene resin and crosslinking agent to improve the impact toughness and modulus of the material.

Benefits of technology

It achieves high impact strength, good rigidity and toughness comprehensive performance, meets the high mechanical performance requirements of communication junction boxes, and reduces material density and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003325320000051
    Figure BDA0005003325320000051
  • Figure BDA0005003325320000061
    Figure BDA0005003325320000061
  • Figure BDA0005003325320000071
    Figure BDA0005003325320000071
Patent Text Reader

Abstract

The invention discloses a high-impact high-modulus polypropylene material as well as a preparation method and application thereof. The polypropylene material comprises the following components in percentage by weight: 20%-30% of first co-polypropylene resin, 20%-30% of second co-polypropylene resin, 3%-8% of polyethylene resin, 5%-10% of a compatilizer, 0.2%-1.0% of a cross-linking agent, 25%-35% of glass fibers and 0.1%-0.5% of a phosphate additive, the melt index of the first co-polypropylene resin is less than that of the second co-polypropylene resin, and the impact strength is greater than that of the second co-polypropylene resin; the polyethylene resin is bimodal polyethylene resin with a molecular weight distribution curve having two peak values; the phosphate auxiliary agent is selected from one or a combination of more of sodium dihydrogen phosphate, monopotassium phosphate and disodium dihydrogen pyrophosphate (Na2H2P2O7). The polypropylene material has high impact strength, high modulus and high mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a high-impact high-modulus polypropylene material and a preparation method and application thereof. Background Art

[0002] The current communications industry is developing rapidly, and the construction of some communications infrastructure such as telecommunications networks, Internet networks, and wireless communication base stations is in full swing. As an important structural material, the communication junction box needs to withstand mechanical stress in a wide range and be used in a harsh physical and chemical environment. When the communication junction box material is used as a structural material, it is generally required to be used outdoors for a long time. Some will be placed in the open air or suspended in the air or buried deep underground. Under harsh conditions of use, the parts are subjected to pressure loads and first undergo elastic deformation, and then as the load time increases, its deformation will gradually increase. When the deformation reaches a certain degree, the parts can no longer be used. As the load increases, the material deforms, the airtightness will fail, and there will be leakage and water ingress, which will cause hidden dangers of communication interruption.

[0003] At present, the materials used in the junction box market include ABS, PC / ABS, ASA, PC+GF (glass fiber), PP+GF and other materials. From the actual use situation, the impact strength of ABS material is low and the light aging resistance is poor. ASA has poor impact strength and PC / ABS material is expensive. PC+GF has poor chemical resistance, low impact resistance and is prone to stress cracking. At present, PP+GF material is more commonly used in the market. PP polypropylene material has low density, high strength, excellent rigidity, hardness and heat resistance, and has good electrical properties, insulation and heat resistance.

[0004] Compared with pure PP, the toughness of glass fiber reinforced PP decreases. For high-toughness applications, the toughness of glass fiber reinforced PP needs to be further improved. Usually, polyolefin elastomer (POE) is added to the composite material system to toughen it. However, after toughening, although the impact strength is improved, the modulus is reduced, which makes it difficult to meet the requirements of the junction box air pressure test standard. That is, it is difficult to obtain polypropylene materials with high impact strength, high modulus, and high mechanical properties at the same time. Summary of the invention

[0005] In view of the shortcomings and deficiencies of the prior art, the present invention provides an improved high-impact high-modulus polypropylene material, which has high impact strength, high modulus and high mechanical properties.

[0006] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A polypropylene material comprises the following components, measured in weight percentage: 20%-30% of a first copolymerized polypropylene resin, 20%-30% of a second copolymerized polypropylene resin, 3%-8% of a polyethylene resin, 5%-10% of a compatibilizer, 0.2%-1.0% of a cross-linking agent, 25%-35% of glass fiber, and 0.1%-0.5% of a phosphate additive; the melt index of the first copolymerized polypropylene resin is less than the melt index of the second copolymerized polypropylene resin, and the impact strength of the first copolymerized polypropylene resin is greater than the impact strength of the second copolymerized polypropylene resin; the polyethylene resin is a bimodal polyethylene resin having a molecular weight distribution curve with two peaks; and the phosphate additive is selected from a combination of one or more of sodium dihydrogen phosphate, potassium dihydrogen phosphate, and disodium dihydrogen pyrophosphate (Na2H2P2O7).

[0008] In the prior art, toughening agents such as polyolefin elastomer (POE) are usually added to polypropylene composite materials for toughening. However, although the impact strength of the obtained polypropylene composite materials is improved, the modulus is reduced, and it is difficult to achieve high impact strength and high modulus at the same time. The inventors of the present application have found through research that by adding a polyethylene resin with a specific structure as a toughening agent to the polypropylene material, adding a phosphate additive and selecting two specific copolymerized polypropylene resins as the base resin, the polypropylene material can have a high modulus while having high impact strength, as well as high other mechanical properties, so that the material can meet the requirements of specific field applications.

[0009] The molecular weight distribution curve of bimodal polyethylene resin shows two obvious peaks. This distribution pattern gives the material unique physical and mechanical properties. The resin contains two polymer chains with different molecular weights at the same time. The lower molecular weight part helps to improve the processing performance of the material, while the higher molecular weight part enhances the melt strength, mechanical properties and stress cracking resistance of the material.

[0010] The present invention imparts super toughness to polypropylene materials by introducing a polyethylene resin with a bimodal structure as a toughening agent. The molecular weight distribution of general polyethylene resins presents a unimodal distribution, while bimodal polyethylene has fewer side chains in the low molecular weight portion. The crystal structure of bimodal polyethylene is different from that of linear polyethylene, and bimodal polyethylene has a unique branching structure and crystal structure. The linear polyethylene structure is arranged linearly, while the crystal structure of the bimodal polyethylene structure is arranged in an undirected manner. When added to polypropylene materials, the polypropylene materials can present better impact toughness. The crystals of the PP polypropylene and bimodal PE polyethylene blending system are restricted, and this restriction can turn the spherulites of PP into wafers, so that the material cannot generate large spherulites, and the crystals are further refined and reduced in size, thereby improving the impact performance.

[0011] The present invention adjusts the acidity and alkalinity of the polypropylene composite material melt by introducing a phosphate additive, so that the pH value of the melt is maintained at a weak acid. The weak acid environment can increase the coupling activity of the glass fiber surface, improve the interface performance between the matrix resin and the inorganic glass fiber, and increase the compatibility of the matrix resin and the inorganic glass fiber, thereby improving the creep resistance and impact performance of the composite material.

[0012] The present invention simultaneously introduces two polypropylene resin matrices, specifically including copolymer polypropylene with high melt index and medium impact resistance and copolymer polypropylene with high impact resistance and low melt index, so that the toughness of the final polypropylene composite material can be improved without reducing the rigidity of the material. The high impact resistance and low melt index polypropylene provides impact toughness to the material, and the high melt index and medium impact resistance polypropylene ensures that the glass fiber is fully dispersed during processing and blending, and the glass fiber can retain a good glass fiber length, thereby significantly improving the tensile strength and rigidity.

[0013] In some embodiments, the crosslinking agent is selected from a combination of one or more of diphenylmethane bismaleimide, meta-phenylene bismaleimide and N-phenyl maleimide.

[0014] In some embodiments, the compatibilizer is maleic anhydride grafted polypropylene; preferably, the grafting rate of maleic anhydride in the maleic anhydride grafted polypropylene is 0.8%-2%.

[0015] Polar groups can be introduced into the molecular chain of polypropylene resin by introducing maleimide crosslinking agents and maleic anhydride grafted polypropylene as compatibilizers. The bonding strength between components mainly depends on the interfacial tension between the components. The smaller the interfacial tension between the components, the greater the bonding strength. The better the compatibility between the components, the greater the bonding strength. Monomers with functional groups and polymers are grafted to introduce functional groups with certain reactivity into some non-polar polymer macromolecule chains, turning them into polar polymers. When the two phases are melted, the intermolecular force will increase, and a certain thickness of interface will be obtained at the junction of the two phases, so that the polymers have a certain compatibility, so that maleic anhydride grafted polypropylene can improve the adhesion between glass fiber and polypropylene matrix resin, improve the tensile properties of the material without reducing the impact properties.

[0016] By introducing maleimide cross-linking agents and maleic anhydride grafted polypropylene as compatibilizers, the bonding force between the substrate and the glass fiber can be improved. The good combination of the glass fiber and the matrix resin prevents the expansion and escape of cracks.

[0017] In some embodiments, the glass fibers are flat glass fibers.

[0018] The introduction of flat glass fiber can improve the strength and modulus of polypropylene composite materials. Compared with conventional glass fiber, flat glass fiber has a flat interface, which can improve longitudinal reinforcement and has good dispersibility. The surface of glass fiber has many polar groups and adhesives. The matrix resin can fully infiltrate and combine with the flat glass fiber, which can improve the pull-out force of the glass fiber when subjected to impact and tensile external forces.

[0019] In some embodiments, the first copolymerized polypropylene resin has a melt index of 1-4 g / 10 min at 230° C. / 2.16 kg and a notched impact strength of 45-55 kJ / m 2 .

[0020] In some embodiments, the second copolymerized polypropylene resin has a melt index of 25-40 g / 10 min at 230° C. / 2.16 kg and a notched impact strength of 15-25 kJ / m 2 .

[0021] In some embodiments, the first copolymerized polypropylene resin and the second copolymerized polypropylene resin are both block copolymerized polypropylene.

[0022] In some embodiments, the polypropylene material further comprises an auxiliary agent selected from one or more combinations of antioxidants, lubricants and colorants.

[0023] In some embodiments, the polypropylene material further comprises, by weight percentage, 0.1%-1.0% antioxidant, 0.1%-1.0% lubricant and 0.1%-1.5% colorant.

[0024] In some embodiments, the antioxidant is selected from one or both of antioxidant 1010 and antioxidant 168.

[0025] In some embodiments, the lubricant is selected from a combination of one or more of stearic acid, metal stearate, and vinyl bisstearamide.

[0026] In some embodiments, the colorant is selected from a combination of one or more of black masterbatch, carbon black, ultramarine, titanium yellow, phthalocyanine blue, and titanium dioxide.

[0027] The present invention also provides a method for preparing the aforementioned polypropylene material, the preparation method comprising the following steps: 1) mixing the first copolymerized polypropylene resin, the second copolymerized polypropylene resin, the polyethylene resin and a compatibilizer, adding other additives and mixing again to obtain a mixture; 2) mixing the mixture and glass fiber, extruding and granulating to obtain the polypropylene material.

[0028] Furthermore, the extrusion is carried out in a twin-screw extruder.

[0029] Furthermore, the glass fiber is added from a fiber adding port of an extruder.

[0030] The present invention also provides the use of the above-mentioned polypropylene material in the field of communications.

[0031] Preferably, the aforementioned polypropylene material is used for communication junction boxes.

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] 1) Good comprehensive performance of rigidity and toughness: At present, the performance of PP+30GF materials for communication junction boxes in the industry is generally low, and the notch impact and bending modulus cannot be taken into account at the same time. Through a good match of the matrix resin, the glass fiber is fully dispersed in the matrix resin, so that the material has an excellent balance of rigidity and toughness.

[0034] 2) Ultra-high impact strength: The impact strength of materials currently used in the market is generally 15kJ / m 2 -20kJ / m 2 The notched impact strength of the material of the present invention can reach 28 kJ / m 2 The above-mentioned injection molded products can withstand the impact of a 16N steel ball falling from a height of 1.5 meters without cracking.

[0035] 3) Low density: In order to pursue rigidity, the industry currently adds too much glass fiber to the material, resulting in a high material density, generally around 1.2g / cm 3 However, this density will cause excessive load on the cables for external communication junction boxes, which poses a great safety hazard. The density of the material of the present invention is less than 1.15g / cm 3 , which can achieve higher mechanical properties with smaller weight.

[0036] 4) Good creep resistance and impact performance: The flexural modulus of the material of the present invention is above 5000 MPa and has good creep resistance.

[0037] 5) Cost reduction and efficiency improvement: POE and other materials are commonly used as toughening agents in communication junction box materials on the market, and the material cost is relatively high. The present invention uses bimodal polyethylene materials instead, which can reduce the material cost. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with the examples. However, the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0039] Example 1

[0040] This embodiment provides a polypropylene material, the raw material composition of which is shown in Table 1 below, and the preparation method thereof is as follows:

[0041] According to the formula in Table 1, first weigh low melt index high impact polypropylene resin (first copolymer polypropylene resin), high melt index medium impact polypropylene resin (second copolymer polypropylene resin) and bimodal polyethylene, place them in a high-speed mixing barrel and stir for 3 minutes, then add other additives and mix for 3 minutes to obtain a first mixture; then weigh glass fiber as the second mixture; when producing granules, add the second mixture from the fiber adding port of the extruder, and use a twin-screw extruder (length-to-diameter ratio of 40:1) to melt extrude and granulate, wherein the extrusion temperature of the twin-screw extruder is 200-250°C, specifically: 200°C for zone 1, 220°C for zone 2, 220°C for zone 3, 220°C for zone 4, 210°C for zone 5, 210°C for zone 6, 220°C for zone 7, 230°C for zone 8, and 240°C for die head; the residence time in the screw of the twin-screw extruder is 5 minutes, the extrusion pressure is 8MPa, and finally the polypropylene material is obtained.

[0042] In Table 1, low melt index high impact polypropylene resin PP1: the melt index is 2.51g / 10min at 230℃ / 2.16kg, and the notched impact strength tested by the cantilever beam notched impact tester is 52kJ / m 2 Block copolymer polypropylene, specifically the commercially available K8003 resin from PetroChina;

[0043] High melt index medium impact polypropylene resin PP2: The melt index is 28.3g / 10min at 230℃ / 2.16kg, and the notched impact strength tested by the cantilever beam notched impact tester is 16kJ / m 2 Block copolymer polypropylene, specifically commercially available K9928 resin;

[0044] Comparison with homopolymer PP3: The melt index is 12g / 10min at 230℃ / 2.16kg, and the notched impact strength tested by the Izod notched impact tester is 3kJ / m 2 Homopolymer polypropylene, specifically commercially available HP500N resin;

[0045] Bimodal polyethylene: The molecular weight distribution curve is bimodal, Sinopec bimodal polyethylene ML2202;

[0046] Ethylene-octene copolymer POE: Dow Chemical 8999;

[0047] PP-g-MAH polypropylene grafted with maleic anhydride: maleic anhydride grafting rate is 1.0%;

[0048] Flat fiberglass: ECS301HP-3-M3;

[0049] Conventional round fiberglass: China Jushi Fiberglass EDR17-2400-988A.

[0050] In Table 1, “-” means that the component is not present.

[0051] Embodiment 2-4

[0052] This embodiment provides a polypropylene material, which is basically the same as that of Embodiment 1, except that the raw material composition is different, as shown in Table 1 below.

[0053] Comparative Examples 1-5

[0054] This comparative example provides a comparative polypropylene material, which is basically the same as Example 1, except that the raw material composition is different, as shown in Table 1 below. In particular, in Comparative Example 1, the type of base resin is changed; in Comparative Example 2, the type of toughening agent is changed; in Comparative Example 3, the type of crosslinking agent is changed; in Comparative Example 4, no phosphate additive is added; and in Comparative Example 5, the type of glass fiber is changed.

[0055] Table 1 Raw material composition of each embodiment and comparative example

[0056]

[0057]

[0058] The performance tests of the polypropylene materials obtained in the embodiments and comparative examples are as follows:

[0059] (1) Tensile strength and elongation at break test: The specimens were prepared by injection molding using an injection molding machine according to ISO527-2 standard;

[0060] (2) Flexural strength and modulus test: The specimens were prepared by injection molding using an injection molding machine in accordance with ISO178 standard;

[0061] (3) Izod notch impact test: The specimens were prepared by injection molding using an injection molding machine in accordance with ISO180 standard;

[0062] (4) Drop ball impact test and material waterproof performance test: A square box with a length of 400 mm and a width of 150 mm is molded by an injection molding machine. The box is sealed and inflated. A 60Kpa, 1KG iron ball is dropped from a height of 1.5 m. The box does not crack after three impacts. It is then immersed in clean water at room temperature and observed for 15 minutes without any bubbles escaping.

[0063] (5) Material density test: Use injection molding machine to prepare samples for testing in accordance with ISO1183 standard;

[0064] (6) Material creep resistance air pressure test: Use an injection molding machine to mold a square box with a length of 400 mm and a width of 150 mm. Fix the periphery with nuts and inflate the box with 60 KPa. Perform 10 cycles of the test at a temperature between -40°C and +65°C. After the test, the air pressure must be ≥55 KPa and the box must not collapse or deform.

[0065] The results are shown in Table 2. OK means that the standard is met, and NG means that the standard is not met.

[0066] Table 2 Performance of each embodiment and comparative example

[0067]

[0068] As can be seen from Table 2, by comparing Example 1 with Comparative Example 1, it can be seen that by selecting a specific copolymerized polypropylene resin as the base resin, the notched impact strength of the material can be improved; by comparing Example 1 with Comparative Example 2, it can be seen that the present invention uses bimodal polyethylene as a toughening agent, which can improve the impact resistance compared with ordinary toughening agents; by comparing Example 1 with Comparative Example 3, it can be seen that the present invention uses a specific cross-linking agent, which can improve the impact strength of the material while improving the tensile strength and modulus compared with ordinary cross-linking agents; by comparing Example 1 with Comparative Example 4, it can be seen that by adding a phosphate additive, the present invention can adjust the pH value of the melt and can further improve the various mechanical properties of the composite material; by comparing Example 1 with Comparative Example 5, it can be seen that the glass fiber with a flat structure can significantly improve the tensile and impact properties of the composite material compared with ordinary glass fibers.

[0069] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention.

[0070] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A polypropylene material, characterized in that: The polypropylene material comprises the following components in weight percentage: 20%-30% of a first copolymerized polypropylene resin, 20%-30% of a second copolymerized polypropylene resin, 3%-8% of a polyethylene resin, 5%-10% of a compatibilizer, 0.2%-1.0% of a cross-linking agent, 25%-35% of glass fiber, and 0.1%-0.5% of a phosphate additive; the melt index of the first copolymerized polypropylene resin is less than the melt index of the second copolymerized polypropylene resin, and the impact strength of the first copolymerized polypropylene resin is greater than the impact strength of the second copolymerized polypropylene resin; the polyethylene resin is a bimodal polyethylene resin having a molecular weight distribution curve with two peaks; and the phosphate additive is selected from a combination of one or more of sodium dihydrogen phosphate, potassium dihydrogen phosphate, and disodium dihydrogen pyrophosphate.

2. The polypropylene material according to claim 1, characterized in that: The crosslinking agent is selected from one or more combinations of diphenylmethane bismaleimide, meta-phenylene bismaleimide and N-phenyl maleimide; and / or the glass fiber is a flat glass fiber.

3. The polypropylene material according to claim 1, characterized in that: The first copolymerized polypropylene resin has a melt index of 1-4 g / 10 min at 230° C. / 2.16 kg, and a notched impact strength of 45-55 kJ / m as tested by an Izod notched impact tester. 2 and / or, the melt index of the second copolymerized polypropylene resin at 230°C / 2.16kg is 25-40g / 10min, and the notched impact strength tested by an Izod notched impact tester is 15-25kJ / m 2 .

4. The polypropylene material according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polypropylene; preferably, the grafting rate of maleic anhydride in the maleic anhydride grafted polypropylene is 0.8%-2%.

5. The polypropylene material according to claim 1, characterized in that: The first copolymerized polypropylene resin and the second copolymerized polypropylene resin are both block copolymerized polypropylene.

6. The polypropylene material according to claim 1, characterized in that: The polypropylene material further comprises an auxiliary agent selected from one or more combinations of antioxidants, lubricants and colorants.

7. The polypropylene material according to claim 6, characterized in that: In terms of weight percentage, the polypropylene material further comprises 0.1%-1.0% antioxidant, 0.1%-1.0% lubricant and 0.1%-1.5% colorant.

8. The polypropylene material according to claim 1, characterized in that: The antioxidant is selected from one or two of antioxidant 1010 and antioxidant 168; and / or the lubricant is selected from a combination of one or more of stearic acid, metal stearate and vinyl bisstearamide; and / or the colorant is selected from a combination of one or more of black masterbatch, carbon black, ultramarine, titanium yellow, phthalocyanine blue and titanium dioxide.

9. The method for preparing the polypropylene material according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: 1) mixing the first copolymerized polypropylene resin, the second copolymerized polypropylene resin, the polyethylene resin and a compatibilizer, adding other additives and mixing again to obtain a mixture; 2) mixing the mixture and glass fiber, extruding and granulating to obtain the polypropylene material.

10. Use of the polypropylene material according to any one of claims 1 to 8 in the field of communications.