SBS elastomer color master batch and preparation method thereof
By using SBS elastomer and modified titanium dioxide in HIPS materials, the problem of single color masterbatch function is solved, the impact strength, flame retardant and antibacterial properties of HIPS materials are improved, and better mechanical properties are achieved and Flame retardant effect.
Patent Information
- Application Number
- CN202411138314.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing masterbatch has a single function and cannot improve the various properties of HIPS masterbatch at the same time, especially in terms of impact strength, toughness and flame retardant properties.
Modified titanium dioxide is prepared by a combination of SBS elastomer and modified titanium dioxide through a two-step reaction of triethoxysilane polyethylene glycol sulfhydryl and allyl triphenyl phosphine bromide. Modified titanium dioxide is used in HIPS materials It has good dispersion and toughening effect, and through uniform dispersion of SBS elastomer and surface modification of modified titanium dioxide, the impact strength and flame retardant properties of the material are improved.
It significantly improves the impact strength and mechanical properties of HIPS materials, enhances the flame retardant and antibacterial properties of composite materials, especially in dark conditions, and improves the overall performance of the material.
Smart Images

Figure BDA0005000022010000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of masterbatches, and in particular relates to an SBS elastomer masterbatch and a preparation method thereof. Background Art
[0002] At present, the main materials for refrigerator liner are acrylonitrile-styrene-butadiene copolymer (ABS) and high-impact polystyrene (HIPS). Among them, the cost of ABS liner is relatively high, and ABS material is not resistant to corrosion by hydrofluorocarbon (HFC) foaming agents or mixed foaming systems containing HFC foaming agents, which is easy to cause cracking and other defects, and there is a high quality risk. Although the performance of unmodified HIPS extruded board materials against the above-mentioned foaming agents has been improved, the cracking ratio of the liner is still relatively high, especially HIPS extruded board materials are usually composed of HPS new materials + masterbatch + scraps. The addition of scraps reduces the impact strength and elongation at break of the board. The deterioration of material properties leads to a greater risk of cracking in the foamed board.
[0003] In order to improve the toughness of the sheet, a toughening agent can be directly added to blend and extrude the sheet, but the extrusion process is difficult to control, and there are problems such as toughening agent agglomeration and uneven dispersion. Toughening masterbatch can also be added to improve this problem. For example, the Chinese patent with publication number CN108219336A discloses HIPS extrusion-grade toughening masterbatch, which is composed of HIPS, titanium dioxide, dispersant, PE wax, coupling agent, and toughening agent. It can improve the flexibility and low-temperature impact strength of HIPS parent material, but there is a problem of single function, and it cannot improve multiple properties of HIPS parent material at the same time. Summary of the invention
[0004] The object of the present invention is to provide an SBS elastomer masterbatch and a preparation method thereof, so as to solve the problem that the existing masterbatch has a single function.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A SBS elastomer masterbatch comprises the following raw materials in parts by weight:
[0007] H IPS (impact resistant polystyrene) 20-25 parts;
[0008] SBS elastomer 50 parts;
[0009] 20-30 parts of modified titanium dioxide;
[0010] 1-2 parts of lubricant;
[0011] 1-3 parts of antioxidant.
[0012] Furthermore, the modified titanium dioxide is obtained by reacting titanium dioxide, triethoxysilane polyethylene glycol mercapto, and allyl triphenylphosphonium bromide in two steps.
[0013] Furthermore, the modified titanium dioxide is prepared by the following steps:
[0014] S1. Add triethoxysilane polyethylene glycol mercapto to an ethanol aqueous solution, adjust the pH value to 3-4 with acetic acid, stir and disperse for 2 hours, add titanium dioxide, ultrasonically disperse for 30 minutes, then heat to 73-76°C, stir and react for 4-6 hours, filter after the reaction, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry to obtain an intermediate product;
[0015] S2. Add the intermediate product into DMF, ultrasonicate for 30 minutes, then add allyl triphenylphosphine bromide and benzoin dimethyl ether, stir and mix for 0.5-1 hour, react under ultraviolet light for 1-2 hours, filter after the reaction, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry to obtain modified titanium dioxide.
[0016] Aiming at the problem that the existing titanium dioxide is easy to agglomerate and has poor dispersibility in HIPS, the present invention provides a modified titanium dioxide. Firstly, the triethoxysilane at the end of the molecular structure of triethoxysilane polyethylene glycol mercapto is used to couple and modify the titanium dioxide, so that an organic modification is formed on the surface of the titanium dioxide and an active mercapto group is introduced to obtain an intermediate product. Then, allyl triphenylphosphonium bromide is grafted on the surface of the intermediate product by mercapto-ene click reaction to obtain the modified titanium dioxide.
[0017] Furthermore, in step S1, the usage ratio of triethoxysilane polyethylene glycol mercapto, ethanol aqueous solution and titanium dioxide is 0.5-1.5g:100-150mL:10g, and the mass fraction of ethanol aqueous solution is 60-80%.
[0018] Furthermore, the titanium dioxide is nano-sized titanium dioxide.
[0019] Furthermore, triethoxysilane polyethylene glycol thiol (Silane-PEG-SH) has a molecular weight of 1-5K and was purchased from Xi'an Kaixin Biotechnology Co., Ltd.
[0020] Furthermore, in step S2, the usage ratio of the intermediate product, DMF, allyl triphenylphosphonium bromide and benzoin dimethyl ether is 10.5-11.5 g: 120-180 mL: 0.8-1.2 g: 0.05-0.1 g.
[0021] Furthermore, the power of the ultraviolet lamp is 300-600W and the wavelength is 365nm.
[0022] Furthermore, the lubricant is at least one of polyethylene wax, N,N'-ethylene bisstearamide (EBS), and stearate.
[0023] Furthermore, the antioxidant is at least one of antioxidant 1010 , antioxidant 1076 , and antioxidant 168 .
[0024] The method for preparing the above-mentioned SBS elastomer masterbatch comprises the following steps:
[0025] Weigh the raw materials according to the ratio, add HIPS, SBS elastomer, modified titanium dioxide, lubricant and antioxidant into the mixer, mix at a temperature of 55-65°C at a high speed of 800-1500r / min for 5-10min to obtain a premix, add the premix from the main feeding port of the twin-screw extruder, melt-extrude and granulate to obtain SBS elastomer masterbatch.
[0026] Furthermore, the barrel temperature of the twin-screw extruder is 185°C in zone 1, 195°C in zone 2, 200°C in zone 3, 205°C in zone 4, 200°C in zone 5, 195°C in zone 6, the head is 185°C, and the screw speed is 315r / min.
[0027] Beneficial effects of the present invention:
[0028] The invention provides an SBS elastomer masterbatch. The SBS in the masterbatch and HIPS contain the same structural unit (styrene), and the two have good compatibility. When the masterbatch is blended with the HIPS base material, in addition to playing a coloring role, the SBS is evenly dispersed in the HIPS, and acts as an effective stress concentration point to induce silver streaks and shear bands to absorb impact energy, thereby preventing the silver streaks from further developing into cracks, and can greatly improve the impact strength of the HIPS material.
[0029] The modified titanium dioxide in the masterbatch also has good dispersibility in the HIPS material, which makes the interface between titanium dioxide and HIPS material good. The presence of the flexible group CSC on the surface of the modified titanium dioxide and the flexible chain of polyethylene glycol enables the modified titanium dioxide to fully exert its strengthening and toughening effects, thus improving the mechanical properties of the composite material.
[0030] In addition, compared with the problem that single titanium dioxide has poor sterilization effect under dark conditions, the modified titanium dioxide of the present invention contains a quaternary phosphonium salt structure on its surface, has good antibacterial effect, is not affected by light factors, is easier to adsorb negatively charged bacteria, and has a wide pH value range. Therefore, the composite material finally prepared also has good antibacterial properties under dark conditions;
[0031] Furthermore, the organic modifiers on the surface of modified titanium dioxide contain flame retardant elements such as N, P, S, and Si, which, combined with the good catalytic carbonization ability of titanium dioxide, ultimately significantly improve the flame retardant properties of the composite material. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The titanium dioxide in the following examples and comparative examples is nano-sized titanium dioxide, triethoxysilane polyethylene glycol thiol (Silane-PEG-SH), purchased from Xi'an Kaixin Biotechnology Co., Ltd.
[0034] Example 1
[0035] A modified titanium dioxide is prepared by the following steps:
[0036] S1. Add 0.5 g triethoxysilane polyethylene glycol thiol (molecular weight 1K) to 100 mL of 60 wt% ethanol aqueous solution, adjust the pH value to 3 with acetic acid, stir and disperse for 2 h, add 10 g titanium dioxide, ultrasonically disperse for 30 min, then heat to 73 ° C, stir and react for 4 h, filter after the reaction, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry to obtain an intermediate product;
[0037] S2. Add 10.5 g of the intermediate product into 120 mL of DMF, and after ultrasonic fractionation for 30 min, add 0.8 g of allyl triphenylphosphine bromide and 0.05 g of benzoin dimethyl ether, stir and mix for 0.5 h, and react under ultraviolet light for 1 h. The power of the ultraviolet lamp is 300 W and the wavelength is 365 nm. After the reaction is completed, filter, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry it to obtain modified titanium dioxide.
[0038] Example 2
[0039] A modified titanium dioxide is prepared by the following steps:
[0040] S1. Add 1.5 g triethoxysilane polyethylene glycol thiol (molecular weight 5K) to 150 mL of 80 wt% ethanol aqueous solution, adjust the pH value to 4 with acetic acid, stir and disperse for 2 h, add 10 g titanium dioxide, ultrasonically disperse for 30 min, then heat to 76 ° C, stir and react for 6 h, filter after the reaction, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry to obtain an intermediate product;
[0041] S2. Add 11.5 g of the intermediate product into 180 mL of DMF, and after ultrasonic fractionation for 30 min, add 1.2 g of allyl triphenylphosphine bromide and 0.1 g of benzoin dimethyl ether, stir and mix for 1 h, and react under ultraviolet light for 2 h. The power of the ultraviolet lamp is 600 W and the wavelength is 365 nm. After the reaction is completed, filter, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry it to obtain modified titanium dioxide.
[0042] Comparative Example 1
[0043] A modified titanium dioxide is prepared by the following steps:
[0044] Add 0.5g triethoxysilane polyethylene glycol mercapto (molecular weight 1K) into 100mL of 60wt% ethanol aqueous solution, and adjust the pH value to 3 with acetic acid. Stir and disperse for 2h, add 10g titanium dioxide, ultrasonically disperse for 30min, then heat to 73°C, stir and react for 4h. After the reaction is completed, filter, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry to obtain modified titanium dioxide.
[0045] Comparative Example 2
[0046] A modified titanium dioxide is prepared by the following steps:
[0047] Add 0.5 g of 3-aminopropyltriethoxysilane to 100 mL of 60 wt% ethanol aqueous solution, adjust the pH value to 3 with acetic acid, stir and disperse for 2 hours, add 10 g of titanium dioxide, ultrasonically disperse for 30 minutes, then heat to 73 ° C, stir and react for 4 hours. After the reaction is completed, filter, wash the filter cake with deionized water and anhydrous ethanol in turn, and then dry to obtain modified titanium dioxide.
[0048] Example 3
[0049] A SBS elastomer masterbatch comprises the following raw materials in parts by weight:
[0050] HIPS (impact resistant polystyrene) 20 parts;
[0051] SBS elastomer 50 parts;
[0052] 20 parts of the modified titanium dioxide of Example 1;
[0053] 1 part of polyethylene wax;
[0054] Antioxidant 10101 parts.
[0055] The preparation method of the above-mentioned SBS elastomer masterbatch comprises the following steps:
[0056] Weigh the raw materials according to the ratio, add HIPS, SBS elastomer, modified titanium dioxide, lubricant and antioxidant into the mixer, mix at a high speed of 800r / min for 5 minutes at a temperature of 55°C to obtain a premix, add the premix from the main feeding port of the twin-screw extruder, melt-extrude and granulate to obtain SBS elastomer masterbatch.
[0057] The barrel temperature of the twin-screw extruder is 185°C in zone 1, 195°C in zone 2, 200°C in zone 3, 205°C in zone 4, 200°C in zone 5, and 195°C in zone 6, the head is 185°C, and the screw speed is 315r / min.
[0058] Example 4
[0059] A SBS elastomer masterbatch comprises the following raw materials in parts by weight:
[0060] H IPS (impact resistant polystyrene) 23 parts;
[0061] SBS elastomer 50 parts;
[0062] 25 parts of the modified titanium dioxide of Example 1;
[0063] 1.5 parts of N,N'-ethylenebisstearamide (EBS);
[0064] 10762 parts of antioxidant.
[0065] The preparation method of the above-mentioned SBS elastomer masterbatch comprises the following steps:
[0066] The raw materials were weighed according to the ratio, and HIPS, SBS elastomer, modified titanium dioxide, lubricant and antioxidant were added into a mixer. The temperature was 60°C and mixed at a high speed of 1200 r / min for 8 minutes to obtain a premix. The premix was added from the main feeding port of a twin-screw extruder, and melt-extruded and granulated to obtain SBS elastomer masterbatch. The parameters of the twin-screw extruder were set the same as those in Example 3.
[0067] Example 5
[0068] A SBS elastomer masterbatch comprises the following raw materials in parts by weight:
[0069] H IPS (impact resistant polystyrene) 25 parts;
[0070] SBS elastomer 50 parts;
[0071] 30 parts of the modified titanium dioxide of Example 2;
[0072] Calcium stearate 2 parts;
[0073] 1683 parts of antioxidants.
[0074] The preparation method of the above-mentioned SBS elastomer masterbatch comprises the following steps:
[0075] The raw materials were weighed according to the ratio, and HIPS, SBS elastomer, modified titanium dioxide, lubricant and antioxidant were added into a mixer at a temperature of 65°C and mixed at a high speed of 1500 r / min for 10 min to obtain a premix. The premix was added from the main feeding port of a twin-screw extruder, and melt-extruded and granulated to obtain SBS elastomer masterbatch. The parameters of the twin-screw extruder were set the same as those in Example 3.
[0076] Comparative Example 3
[0077] A SBS elastomer masterbatch is prepared based on Example 3, except that the "modified titanium dioxide" in Example 3 is replaced by the product in Comparative Example 1, and the remaining raw materials, parameters and processes are the same as those in Example 3.
[0078] Comparative Example 4
[0079] A SBS elastomer masterbatch is prepared based on Example 3, except that the "modified titanium dioxide" in Example 3 is replaced by the product in Comparative Example 2, and the remaining raw materials, parameters and processes are the same as those in Example 3.
[0080] The SBS elastomer masterbatches prepared in Examples 3 to 5 and Comparative Examples 3 to 4 were added to a mixer with a HIPS masterbatch at a mass ratio of 1:3, and mixed at a high speed of 1500 r / min for 10 min at a temperature of 65°C to obtain a premix. The premix was added from the main feeding port of a twin-screw extruder and melt-extruded to form granules. The barrel temperature of the twin-screw extruder was 185°C in zone 1, 195°C in zone 2, 200°C in zone 3, 205°C in zone 4, 200°C in zone 5, and 195°C in zone 6. The die head was 185°C and the screw speed was 315 r / min to obtain a composite material. The composite material was injection molded into a standard specimen at 180-200°C using an injection molding machine and the performance was tested:
[0081] The tensile properties are tested according to GB / T 1040.1-2006, and the tensile rate is 50mm / min;
[0082] Notched impact strength is tested according to GB / T 1843-2008;
[0083] Vertical burning performance is tested according to UL94;
[0084] The antibacterial test is carried out in accordance with the standard GB / T 31402-2015 "Test Method for Antibacterial Performance of Plastic Surfaces". Specifically, each group of samples is placed in a natural environment for 1000 hours before conducting an antibacterial test. The lighting conditions are 50% light + 50% darkness. Specifically, within 24 hours of bacterial culture, there are 12 hours of natural light time and 12 hours of darkness time. The bacterial species are Escherichia coli and Staphylococcus aureus.
[0085] The results are shown in Table 1:
[0086] Table 1
[0087]
[0088] It can be seen from the data recorded in Table 1 that, compared with Comparative Example 3 and Comparative Example 4, the SBS elastomer masterbatch prepared in Example 3, Example 4 and Example 5 has a better overall effect on the HIPS masterbatch. Specifically, it can be seen from the test results of Comparative Example 3 and Example 3 that the absence of allyl triphenylphosphine bromide in the preparation process of the modified titanium dioxide will cause the flame retardant and antibacterial properties of the composite material to be significantly reduced. It can be seen from the test results of Comparative Example 4 and Example 3 that the modified titanium dioxide prepared by the present invention has a better toughening effect on the HIPS masterbatch than the existing coupling agent-modified titanium dioxide, and imparts good flame retardant and antibacterial properties to the composite material.
[0089] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0090] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A SBS elastomer masterbatch, characterized in that: It includes the following raw materials in parts by weight: HIPS 20-25 copies; SBS elastomer 50 parts; 20-30 parts of modified titanium dioxide; 1-2 parts of lubricant; 1-3 parts of antioxidant; The modified titanium dioxide is obtained by reacting titanium dioxide, triethoxysilane polyethylene glycol mercapto and allyl triphenylphosphonium bromide in two steps.
2. The SBS elastomer masterbatch according to claim 1, characterized in that: The modified titanium dioxide is prepared by the following steps: S1. Add triethoxysilane polyethylene glycol thiol to an ethanol aqueous solution, adjust the pH value to 3-4 with acetic acid, stir and disperse for 2 hours, add titanium dioxide, ultrasonically disperse for 30 minutes, stir and react at 73-76° C. for 4-6 hours, filter after the reaction, wash the filter cake and dry it to obtain an intermediate product; S2. Add the intermediate product into DMF, ultrasonicate for 30 min, add allyl triphenylphosphine bromide and benzoin dimethyl ether, stir and mix for 0.5-1 h, react under ultraviolet light for 1-2 h, filter after the reaction, wash and dry the filter cake to obtain modified titanium dioxide.
3. The SBS elastomer masterbatch according to claim 2, characterized in that: In step S1, the usage ratio of triethoxysilane polyethylene glycol mercapto, ethanol aqueous solution and titanium dioxide is 0.5-1.5g:100-150mL:10g, and the mass fraction of ethanol aqueous solution is 60-80%.
4. The SBS elastomer masterbatch according to claim 2, characterized in that: In step S2, the usage ratio of the intermediate product, DMF, allyl triphenylphosphonium bromide and benzoin dimethyl ether is 10.5-11.5 g: 120-180 mL: 0.8-1.2 g: 0.05-0.1 g.
5. A method for preparing the SBS elastomer masterbatch according to any one of claims 1 to 4, characterized in that: The following steps are involved: Weigh the raw materials according to the ratio, add HIPS, SBS elastomer, modified titanium dioxide, lubricant and antioxidant into the mixer, mix at 55-65°C for 5-10 minutes to obtain a premix, add the premix from the main feeding port of the twin-screw extruder, melt-extrude and granulate to obtain SBS elastomer masterbatch.
6. The method for preparing the SBS elastomer masterbatch according to claim 5, characterized in that: The barrel temperature of the twin-screw extruder is 185°C in zone 1, 195°C in zone 2, 200°C in zone 3, 205°C in zone 4, 200°C in zone 5, and 195°C in zone 6, the head is 185°C, and the screw speed is 315r / min.