Aluminum-silicon composite material for electronic packaging and preparation method thereof
Through the combination of modified phenolic resin, hydroxylated silicon carbide whiskers and modified aluminum powder, chemical bonding reactions are used to solve the problem of poor process stability of aluminum-silicon composite materials, and its thermal conductivity, heat resistance and tensile resistance are improved , simplifies the process and reduces costs.
Patent Information
- Application Number
- CN202410890533.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing aluminum-silicon composite materials have poor process stability, which affects their thermal conductivity, heat resistance and tensile resistance.
Modified phenolic resin, hydroxylated silicon carbide whiskers and modified aluminum powder are used to form an aluminum-silicon composite material through ultrasonic treatment and hot pressing forming process, and the chemical bonding reaction of hydroxylated silicon carbide with modified aluminum powder and phenolic resin is used. , the thermal conductivity and tensile strength of the reinforced material.
The thermal conductivity, heat resistance and tensile properties of aluminum-silicon composite materials are improved, the process flow is simplified, the cost is reduced, and the material stability is improved.
Smart Images

Figure BDA0004927364110000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electronic packaging material preparation, and in particular, relates to an aluminum-silicon composite material for electronic packaging and a preparation method thereof. Background Art
[0002] Electronic packaging materials are base materials used to carry electronic devices and their interconnections, and play the role of heat dissipation, mechanical support, sealing, environmental protection, signal transmission and shielding. With the development of microelectronics technology, electronic components have higher integration, faster operating speed and larger capacity. This leads to increased circuit heat generation and increased operating temperature. The failure rate of electronic devices increases sharply with the increase in operating temperature. Basically, for every 10°C increase in operating temperature, the life of semiconductor devices will decrease by one third. Heat dissipation and cooling of electronic devices are usually achieved by heat sinks, radiators and electronic packaging materials. Research and development of electronic packaging materials with high thermal conductivity, low thermal expansion coefficient and good comprehensive performance has become a key technology in the field of electronic packaging and has affected the development of the electronics industry.
[0003] Invention patent CN107540378B discloses a method for preparing a silicon carbide / aluminum composite material: dissolving phenolic resin powder in anhydrous ethanol; adding SiC powder to the resulting solution and stirring evenly at 40-60°C; sequentially adding SiO2 aerogel powder and Al powder to the resulting solution, stirring evenly and then ball milling for 10-12h; drying the slurry obtained after ball milling, granulating and screening, and then pressing the obtained granular powder into a shape to obtain a green body; placing a certain mass of Al2O3 plates on the green body, reacting and sintering at 900-000°C in vacuum for 1-2h to obtain a SiC green body; gaseous aluminum infiltration of the SiC green body at 900-1100°C in vacuum for 0.5-1h, and then naturally cooling to obtain a silicon carbide / aluminum composite material. The SiC / Al composite material prepared by the invention has good mechanical strength, thermal conductivity and low thermal expansion coefficient, but it has problems such as difficult process control and poor stability, which ultimately affect the performance of the material. Summary of the invention
[0004] The purpose of the present invention is to provide to solve the following technical problems:
[0005] The purpose is to improve the poor process stability of the prior art and to enhance the thermal conductivity, heat resistance and tensile strength of aluminum silicon composite materials used for electronic packaging.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] An aluminum-silicon composite material for electronic packaging comprises the following raw materials in parts by weight: 20-30 parts of modified phenolic resin, 1.5-2.0 parts of p-toluenesulfonic acid, 70-90 parts of N,N-dimethylformamide, 20-30 parts of hydroxylated silicon carbide whiskers and 30-40 parts of modified aluminum powder;
[0008] The preparation method of the aluminum-silicon composite material for electronic packaging comprises the following steps:
[0009] The modified phenolic resin, p-toluenesulfonic acid and N, N-dimethylformamide are added into a three-necked flask, and ultrasonically treated for 10-15 minutes, and hydroxylated silicon carbide whiskers and modified aluminum powder are added, and the temperature is raised to 65-70°C, and the rotation speed is 600-700rpm, and the reaction is stirred for 5-6 hours. After the reaction is completed, a preform is obtained, and the obtained preform is hot-pressed and stress-relieved annealed to obtain an aluminum silicon composite material for electronic packaging. N, N-dimethylformamide is used as a reaction solvent and p-toluenesulfonic acid is used as a catalyst. The hydroxyl groups in the hydroxy silicon carbide whiskers react with (2-methyl-2-propylene) succinic anhydride on the surface of the modified aluminum powder to undergo a ring-opening esterification reaction. After the reaction is completed, the remaining hydroxyl groups on the remaining hydroxy silicon carbide continue to undergo an esterification reaction with the carboxyl groups generated by the reaction and the carboxyl groups on the modified phenolic resin to obtain a preform, and the preform is pressed and formed to obtain the aluminum silicon composite material for electronic packaging.
[0010] Furthermore, the method for preparing hydroxy silicon carbide whiskers comprises the following steps:
[0011] The silicon carbide whisker is immersed in a 30wt% hydrofluoric acid solution for 24 hours, and then washed with deionized water for several times to obtain acid-treated silicon carbide whiskers, wherein the amount ratio of the silicon carbide whisker to the 30wt% hydrofluoric acid solution is 10g:150-200mL, and the obtained acid-treated silicon carbide whisker is immersed in 30wt% hydrogen peroxide for 40-70min to obtain hydroxylated silicon carbide whiskers, wherein the amount ratio of the acid-treated silicon carbide whisker to the 30wt% hydrogen peroxide is 8g:120-150mL.
[0012] Furthermore, the preparation method of the modified phenolic resin comprises the following steps:
[0013] Carboxylated nitrile rubber, phenol and dioctyl phthalate are added into a three-necked flask, stirred evenly, heated to 60-65° C., hydrofluoric acid is added under stirring, and the reaction is kept warm for 5-6 hours. After the reaction is completed, the temperature is raised to 100-120° C., 25-30wt% formaldehyde aqueous solution is added dropwise, stirred for reaction for 2-3 hours, dehydrated and dried, and cooled to room temperature to obtain a modified phenolic resin, wherein the amount ratio of carboxylated nitrile rubber, phenol, dioctyl phthalate, hydrofluoric acid and 25-30wt% formaldehyde aqueous solution is 50-60mL:20-30g:0.5-1g:0.6-1mL:15-22mL, dioctyl phthalate is used as a toughening agent, hydrofluoric acid is used as a catalyst, carboxylated nitrile rubber and phenol undergo Friedel-Crafts alkylation reaction, and then polymerized with formaldehyde to obtain a modified phenolic resin with high toughness and good heat resistance.
[0014] Furthermore, the preparation method of the modified aluminum powder comprises the following steps:
[0015] Step A1, add styrene, (2-methyl-2-propenyl) succinic anhydride, butyl acrylate and 2-hydroxyethyl methacrylate into a three-necked flask, add 9 / 10 volume portion of mixed solution a dropwise while stirring, raise the temperature to 120-130° C., stir and react for 1-1.5 hours, keep warm for 1 hour, add the remaining 1 / 10 volume portion of mixed solution a, continue to keep warm and react for 3 hours, cool, add n-hexane, filter the precipitate, and vacuum dry at 55° C. for 10 hours to obtain a modified polymer;
[0016] The amount ratio of styrene, (2-methyl-2-propenyl) succinic anhydride, butyl acrylate, 2-hydroxyethyl methacrylate, mixed solution a and n-hexane is 13-14 g: 4-5 g: 4-5 g: 5.2-6.5 g: 30-35 mL: 55-65 mL, the amount ratio of xylene and dibenzoyl peroxide in the mixed solution a is 20-22.5 mL: 0.3-0.4 g, and the benzoyl peroxide in the mixed solution a is used as a catalyst, and methyl methacrylate, (2-methyl-2-propenyl) succinic anhydride, butyl acrylate and 2-hydroxyethyl methacrylate are used as monomers to undergo copolymerization to obtain a modified polymer;
[0017] Step A2, add the pretreated aluminum powder and ethanol into a three-necked flask, stir evenly, heat to 40-60°C, add the mixed solution b dropwise through a constant pressure dropping funnel, control the dropping speed to 1 drop / second, and after the dropping is completed, keep warm and stir for 1-4h, end the reaction, filter, wash 2-3 times, and dry to obtain modified aluminum powder;
[0018] Among them, the dosage ratio of pretreated aluminum powder, ethanol and mixed liquid b is 1-2g:30-50mL:35-40mL, the dosage ratio of ethanol, modified polymer, ammonia water and distilled water in the mixed liquid b is 30mL:6g:2-4mL:3-6mL, the hydroxyl groups in the modified polymer form hydrogen bonds with the hydroxyl groups on the surface of the aluminum powder, and then a condensation reaction occurs to adsorb on the surface of the aluminum powder, thereby forming a dense protective film on the surface of the aluminum powder.
[0019] Furthermore, the preparation method of pretreated aluminum powder comprises the following steps:
[0020] Aluminum powder, 9-10wt% phosphoric acid aqueous solution and 30-35wt% ethanol aqueous solution are added into a three-necked flask, mechanically stirred at 600-800rpm for 12-16h, and dried to obtain pretreated aluminum powder, wherein the amount ratio of aluminum powder, 9-10wt% phosphoric acid and 30-35wt% ethanol aqueous solution is 1.5-2g:10mL:40mL. Since aluminum is chemically active and easily reacts with oxygen or water, a thin layer of aluminum oxide is covered on the surface of aluminum powder in an aerobic environment. Dry Al2O3 is Lewis acid, which is easy to absorb water molecules in a humid environment. Hydroxyl groups react with metal ions in the form of Al-OH, A lO-OH and other forms of combination, so that the aluminum surface has hydroxyl groups. In the process of producing aluminum powder, an inert liquid carrier (mainly fatty acid or ester) is often added as a lubricant. The surface of the obtained ultrafine flaky aluminum particles is coated with a thin layer of lubricant, which can not only prevent the aluminum flakes from agglomerating, but also protect the surface of the aluminum powder from acid or alkali corrosion, but also form a steric hindrance to the hydroxyl groups on the surface of the aluminum powder. The hydroxyl groups on the surface of the aluminum powder can be exposed through the pretreatment process.
[0021] Furthermore, the temperature of the hot pressing molding is 800-1500°C.
[0022] Furthermore, the stress relief annealing is performed in an inert atmosphere at a temperature of 600-1200° C., and the stress relief annealing time is 0.5-2 h.
[0023] Furthermore, the usage ratio of hydroxylated silicon carbide whisker, modified aluminum powder and N,N-dimethylformamide in the mixed monomer is 3-5g:5-6g:50-60mL.
[0024] Furthermore, the carboxylated nitrile rubber is any one of XR-3270 and TL910.
[0025] Furthermore, the average particle size of the aluminum powder is 20-30 μm.
[0026] Beneficial effects of the present invention:
[0027] (1) In order to improve the thermal conductivity, heat resistance and tensile strength of the aluminum-silicon composite material for electronic packaging, the present invention adds modified aluminum powder. The hydroxyl groups in the modified polymer in the modified aluminum powder can form hydrogen bonds with the hydroxyl groups on the surface of the aluminum powder, and then undergo a condensation reaction to be adsorbed on the surface of the aluminum powder. By forming a dense protective film on the surface of the aluminum powder, the (2-methyl-2-propenyl) succinic anhydride in the modified polymer coated on the surface of the aluminum powder chemically bonds with the hydroxyl groups on the hydroxy silicon carbide whiskers through a ring-opening esterification reaction, and the silicon carbide whiskers with strong heat resistance are tightly combined with the aluminum powder with high thermal conductivity, which not only effectively realizes the uniform dispersion of the aluminum powder, but also further enhances the thermal conductivity and tensile strength of the aluminum-silicon composite material. In addition, the hydroxyl groups on the hydroxy silicon carbide continue to undergo an esterification reaction with the carboxyl groups on the modified phenolic resin, further enhancing the heat resistance of the aluminum-silicon composite material for electronic packaging.
[0028] (2) The present invention uses modified aluminum powder as a substrate, obtains a preform by chemically bonding hydroxy silicon carbide whiskers and modified phenolic resin, and then presses the preform into an aluminum silicon composite material through a hot pressing process. Compared with traditional processing technology, the process is simpler and the cost is lower. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] The present embodiment provides a method for preparing pretreated aluminum powder, comprising the following steps:
[0032] 1.5 g aluminum powder, 10 mL 9 wt % phosphoric acid aqueous solution and 40 mL 30 wt % ethanol aqueous solution were added into a three-necked flask, mechanically stirred at 600 rpm for 12 h, and dried to obtain pretreated aluminum powder.
[0033] Example 2
[0034] The present embodiment provides a method for preparing pretreated aluminum powder, comprising the following steps:
[0035] 2 g of aluminum powder, 10 mL of 10 wt% phosphoric acid and 40 mL of 35 wt% ethanol aqueous solution were added into a three-necked flask, mechanically stirred at 800 rpm for 16 h, and dried to obtain pretreated aluminum powder.
[0036] Example 3
[0037] The present embodiment provides a method for preparing a modified aluminum powder, comprising the following steps:
[0038] Step A1, 13g styrene, 4g (2-methyl-2-propenyl) succinic anhydride, 4g butyl acrylate and 5.2g 2-hydroxyethyl methacrylate were added to a three-necked flask, 18mL of mixed solution a was added dropwise while stirring, the temperature was raised to 120°C, stirred for reaction for 1h, kept warm for 1h, 2mL of mixed solution a was added, the reaction was continued for 3h, cooled, 55mL of n-hexane was added, the precipitate was filtered, and vacuum dried at 55°C for 10h to obtain a modified polymer, wherein the amount ratio of xylene to dibenzoyl peroxide in the mixed solution a was 20mL:0.3-0.4g;
[0039] Step A2, add 1g of the pretreated aluminum powder prepared in Example 1 and 30mL of ethanol into a three-necked flask, stir evenly, heat to 40°C, add 35mL of mixed solution b through a constant pressure dropping funnel, control the dropping speed to 1 drop / second, after the addition is completed, keep warm and stir for 1h, end the reaction, filter, wash twice, and dry to obtain modified aluminum powder, the amount ratio of ethanol, modified polymer, ammonia water and distilled water in the mixed solution b is 30mL:6g:2mL:3mL.
[0040] Example 4
[0041] The present embodiment provides a method for preparing a modified aluminum powder, comprising the following steps:
[0042] Step A1, 14g styrene, 5g (2-methyl-2-propenyl) succinic anhydride, 5g butyl acrylate and 65mL 2-hydroxyethyl methacrylate were added to a three-necked flask, 20.25mL of mixed solution a was added dropwise while stirring, the temperature was raised to 130°C, stirred for reaction for 1.5h, kept warm for 1h, 2.25mL of mixed solution a was added, the reaction was continued for 3h, cooled, 65mL of n-hexane was added, the precipitate was filtered, and vacuum dried at 55°C for 10h to obtain a modified polymer, wherein the amount ratio of xylene to dibenzoyl peroxide in the mixed solution a was 22.5mL:0.4g;
[0043] Step A2, add 2g of the pretreated aluminum powder prepared in Example 2 and 50mL of ethanol into a three-necked flask, stir evenly, heat to 60°C, add 40mL of mixed solution b through a constant pressure dropping funnel, control the dropping speed to 1 drop / second, after the addition is completed, keep warm and stir for 4h, end the reaction, filter, wash 3 times, and dry to obtain modified aluminum powder, the amount ratio of ethanol, modified polymer, ammonia water and distilled water in the mixed solution b is 30mL:6g:4mL:6mL.
[0044] Example 5
[0045] This embodiment provides a method for preparing a modified phenolic resin, comprising the following steps:
[0046] Add 50 mL of carboxylated nitrile rubber, 20 g of phenol and 0.5 g of dioctyl phthalate into a three-necked flask, stir evenly, heat to 60°C, add 0.6 mL of hydrofluoric acid while stirring, and keep warm for 5 hours. After the reaction is completed, heat to 100°C, add 15 mL of 25 wt% formaldehyde aqueous solution dropwise, stir for 2 hours, dehydrate and dry, and cool to room temperature to obtain modified phenolic resin.
[0047] Example 6
[0048] This embodiment provides a method for preparing a modified phenolic resin, comprising the following steps:
[0049] Add 60mL of carboxylated nitrile rubber, 30g of phenol and 1g of dioctyl phthalate into a three-necked flask, stir evenly, heat to 65°C, add 1mL of hydrofluoric acid while stirring, and keep warm for 6h. After the reaction is completed, heat to 120°C, add 22mL of 30wt% formaldehyde aqueous solution dropwise, stir for 3h, dehydrate and dry, and cool to room temperature to obtain modified phenolic resin.
[0050] Example 7
[0051] This embodiment provides a method for preparing hydroxy silicon carbide whiskers, comprising the following steps:
[0052] 10 g of silicon carbide whiskers were soaked in 150 mL of 30 wt% hydrofluoric acid solution for 24 h, and then washed with deionized water for several times to obtain acid-treated silicon carbide whiskers. 8 g of the acid-treated silicon carbide whiskers were soaked in 120 mL of 30 wt% hydrogen peroxide for 40 min to obtain hydroxylated silicon carbide whiskers.
[0053] Example 8
[0054] This embodiment provides a method for preparing hydroxy silicon carbide whiskers, comprising the following steps:
[0055] 10 g of silicon carbide whiskers were soaked in 200 mL of 30 wt% hydrofluoric acid solution for 24 h, and then washed with deionized water for several times to obtain acid-treated silicon carbide whiskers. 8 g of the acid-treated silicon carbide whiskers were soaked in 150 mL of 30 wt% hydrogen peroxide for 70 min to obtain hydroxylated silicon carbide whiskers.
[0056] Example 9
[0057] This embodiment provides an aluminum-silicon composite material for electronic packaging, comprising the following raw materials in parts by weight: 20 parts of the modified phenolic resin prepared in Example 5, 1.5 parts of p-toluenesulfonic acid, 70 parts of N,N-dimethylformamide, 20 parts of the hydroxylated silicon carbide whiskers prepared in Example 7, and 30 parts of the modified aluminum powder prepared in Example 3;
[0058] The preparation method of the aluminum-silicon composite material for electronic packaging comprises the following steps:
[0059] Step A1, add modified phenolic resin, p-toluenesulfonic acid and N, N-dimethylformamide into a three-necked flask, and ultrasonically treat for 10 minutes, add hydroxylated silicon carbide whiskers and modified aluminum powder, raise the temperature to 65°C, rotate at 600 rpm, and stir to react for 5 hours. After the reaction is completed, a preform is obtained, and the obtained preform is hot-pressed at 800°C, and stress-relieved annealed at 600°C for 0.5 hours to obtain an aluminum-silicon composite material for electronic packaging.
[0060] Example 10
[0061] This embodiment provides an aluminum-silicon composite material for electronic packaging, comprising the following raw materials in parts by weight: 30 parts of the modified phenolic resin prepared in Example 5, 2.0 parts of p-toluenesulfonic acid, 90 parts of N,N-dimethylformamide, 30 parts of the hydroxylated silicon carbide whiskers prepared in Example 8, and 40 parts of the modified aluminum powder prepared in Example 4;
[0062] The preparation method of the aluminum-silicon composite material for electronic packaging comprises the following steps:
[0063] Step A1, add modified phenolic resin, p-toluenesulfonic acid and N, N-dimethylformamide into a three-necked flask, and ultrasonically treat for 15 minutes, add hydroxylated silicon carbide whiskers and modified aluminum powder, raise the temperature to 70°C, and stir the reaction at a speed of 700 rpm for 6 hours. After the reaction is completed, a preform is obtained. The obtained preform is hot-pressed at 1500°C and stress-relieved at 1200°C for 2 hours to obtain an aluminum-silicon composite material for electronic packaging.
[0064] Comparative Example 1
[0065] The 9 wt % phosphoric acid aqueous solution in Example 1 was removed, and the remaining raw materials and preparation process were the same as in Example 1.
[0066] Comparative Example 2
[0067] The pretreated aluminum powder in Example 3 was replaced by the material in Comparative Example 1, and the remaining raw materials and preparation process were the same as in Example 3.
[0068] Comparative Example 3
[0069] The (2-methyl-2-propenyl)succinic anhydride in Example 4 was removed, and the remaining raw materials and preparation process were the same as in Example 4.
[0070] Comparative Example 4
[0071] The modified polymer in Example 4 was removed, and the remaining raw materials and preparation process were the same as in Example 4.
[0072] Comparative Example 5
[0073] The carboxyl nitrile rubber in Example 5 is removed, and the remaining raw materials and preparation process are the same as in Example 5.
[0074] Comparative Example 6
[0075] The modified phenolic resin in Example 9 was removed, and the remaining raw materials and preparation process were the same as in Example 9.
[0076] Comparative Example 7
[0077] The modified phenolic resin in Example 9 was replaced by the material prepared in Comparative Example 5, and the remaining raw materials and preparation process were the same as in Example 9.
[0078] Comparative Example 8
[0079] The modified aluminum powder in Example 9 is replaced by the material prepared in Comparative Example 2, and the remaining raw materials and preparation process are the same as in Example 9.
[0080] Comparative Example 9
[0081] The modified aluminum powder in Example 9 is replaced by the material prepared in Comparative Example 3, and the remaining raw materials and preparation process are the same as in Example 9.
[0082] Comparative Example 10
[0083] The modified aluminum powder in Example 10 is replaced by the material prepared in Comparative Example 4, and the remaining raw materials and preparation process are the same as in Example 10.
[0084] Performance Testing
[0085] Tensile strength: Using tensile machine, model E45.105, loading rate 1mm / s.
[0086] Thermal expansion coefficient: using a thermal expansion instrument, model DIL, Netzsche, STA-449-F3, heating temperature to 400 ° C, heating rate 5 ° C / min. Sample size diameter 5.5 × 25 mm.
[0087] Thermal conductivity: Using a laser thermal conductivity meter, model LFA-467, the heating temperature was 400°C, the heating rate was 5°C / min, the thermal diffusion coefficient D of the material was obtained, and the thermal conductivity of the material was calculated. The test results are shown in Table 1:
[0088] Table 1
[0089]
[0090] It can be seen from Table 1 that, compared with Comparative Examples 6-10, the aluminum-silicon composite materials for electronic packaging prepared in Examples 9-10 have excellent heat resistance, thermal conductivity and tensile strength.
[0091] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0092] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An aluminum-silicon composite material for electronic packaging, Features , including the following raw materials in parts by weight: 20-30 parts of modified phenolic resin, 1.5-2.0 parts of p-toluenesulfonic acid, 70-90 parts of N, N-dimethylformamide, 20-30 parts of hydroxylated silicon carbide whiskers and 30-40 parts of modified aluminum powder; The preparation method of the modified phenolic resin comprises the following steps: Add carboxylated nitrile rubber, phenol and dioctyl phthalate into a three-necked flask, stir evenly, heat to 60-65°C, add hydrofluoric acid while stirring, keep warm for 5-6 hours, after the reaction is finished, heat to 100-120°C, add 25-30wt% formaldehyde aqueous solution dropwise, react for 2-3 hours, after the reaction is finished, dehydrate and dry, cool to room temperature to obtain modified phenolic resin.
2. The aluminum-silicon composite material for electronic packaging according to claim 1, It is characterized in that The preparation method of hydroxylated silicon carbide whiskers comprises the following steps: The silicon carbide whiskers were immersed in a 30wt% hydrofluoric acid solution for 24 hours, and then washed with deionized water for several times to obtain acid-treated silicon carbide whiskers, wherein the mass ratio of the silicon carbide whiskers to the 30wt% hydrofluoric acid solution was 10g:150-200mL, and the obtained acid-treated silicon carbide whiskers were immersed in 30wt% hydrogen peroxide for 40-70min to obtain hydroxylated silicon carbide whiskers.
3. The aluminum-silicon composite material for electronic packaging according to claim 2, It is characterized in that The amount ratio of silicon carbide whisker to 30wt% hydrofluoric acid solution is 10g:150-200mL, and the mass ratio of acid-treated silicon carbide whisker to 30wt% hydrogen peroxide is 8g:120-150mL.
4. The aluminum-silicon composite material for electronic packaging according to claim 1, It is characterized in that The usage ratio of carboxyl nitrile rubber, phenol, dioctyl phthalate, hydrofluoric acid and 25-30wt% formaldehyde aqueous solution is 50-60mL:20-30g:0.5-1g:0.6-1mL:15-22mL.
5. The aluminum-silicon composite material for electronic packaging according to claim 1, It is characterized in that The preparation method of modified aluminum powder comprises the following steps: Step A1, add styrene, (2-methyl-2-propenyl) succinic anhydride, butyl acrylate and 2-hydroxyethyl methacrylate into a three-necked flask, add 9 / 10 volume portion of mixed solution a dropwise while stirring, raise the temperature to 120-130° C., stir and react for 1-1.5 hours, keep warm for 1 hour, add the remaining 1 / 10 volume portion of mixed solution a, continue to keep warm and react for 3 hours, cool, add n-hexane, filter the precipitate, and vacuum dry at 55° C. for 10 hours to obtain a modified polymer; Step A2, add the pretreated aluminum powder and ethanol into a three-necked flask, stir evenly, heat to 40-60°C, add the mixed solution b dropwise through a constant pressure dropping funnel, control the dropping speed to 1 drop / second, and after the addition is completed, keep warm and stir for 1-4 hours. After the reaction is completed, filter, wash 2-3 times, and dry to obtain modified aluminum powder.
6. The aluminum-silicon composite material for electronic packaging according to claim 5, It is characterized in that In step A1, the amount ratio of styrene, (2-methyl-2-propenyl) succinic anhydride, butyl acrylate, 2-hydroxyethyl methacrylate, mixed solution a and n-hexane is 13-14g: 4-5g: 4-5g: 5.2-6.5g: 20-22.5mL: 55-65mL, the amount ratio of xylene and dibenzoyl peroxide in the mixed solution a is 20-22.5mL: 0.3-0.4g, and in step A2, the amount ratio of pretreated aluminum powder, ethanol and mixed solution b is 1-2g: 30-50mL: 35-40mL, and the amount ratio of ethanol, modified polymer, ammonia water and distilled water in the mixed solution b is 30mL: 6g: 2-4mL: 3-6mL.
7. The aluminum-silicon composite material for electronic packaging according to claim 5, It is characterized in that The preparation method of pre-treated aluminum powder comprises the following steps: Aluminum powder, 9-10 wt % phosphoric acid aqueous solution and 30-35 wt % ethanol aqueous solution are added into a three-necked flask, mechanically stirred at 600-800 rpm for 12-16 hours, and dried to obtain pretreated aluminum powder.
8. The aluminum-silicon composite material for electronic packaging according to claim 7, It is characterized in that The usage ratio of aluminum powder, 9-10wt% phosphoric acid and 30-35wt% ethanol aqueous solution is 1.5-2g:10mL:40mL.
9. A method for preparing the aluminum-silicon composite material for electronic packaging according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Add modified phenolic resin, p-toluenesulfonic acid and N,N-dimethylformamide into a three-necked flask, and perform ultrasonic treatment for 10-15 minutes. Add hydroxylated silicon carbide whiskers and modified aluminum powder, raise the temperature to 65-70°C, and stir the reaction at a speed of 600-700 rpm for 5-6 hours. After the reaction is completed, a preform is obtained. The obtained preform is hot-pressed and stress-relieved to obtain an aluminum-silicon composite material for electronic packaging.
Citation Information
Cited By
Modified multi-walled carbon nanotube / silicon carbide / cellulose nanocrystal heat-conducting composite material and preparation method thereof
CN117659516A