Low-mold-temperature high-crystallization polyphenylene sulfide composite modified material as well as preparation method and application thereof

By copolymerizing the modified material with polyphenylene sulfide and polyethylene terephthalate, a high crystallinity polyphenylene sulfide composite modified material is formed, which solves the problem of low crystallinity at low mold temperature and achieves low temperature The preparation of high-performance polyphenylene sulfide parts at mold temperature reduces costs and improves material performance.

CN118909438AInactive Publication Date: 2024-11-08GUANGDONG HONGSU TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411119416.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing polyphenylene sulfide materials have low crystallinity when molded at low mold temperature, resulting in poor appearance and poor performance of the parts, and the traditional high mold temperature process is costly and difficult to use.

Method used

The modified material is copolymerized with polyphenylene sulfide and polyethylene terephthalate, and formed by liquid-liquid separation phase and island-like spherical crystal nucleus, combining compatibility agents and coupling agents to improve the crystallinity and performance of the material.

Benefits of technology

Achieve high crystallinity (52-56%) under low mold temperature conditions, improve the appearance, mechanical, physical, heat resistance and electrical properties of the material, reduce mold and processing costs, and improve the quality of the parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909438A_ABST
    Figure CN118909438A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polyphenylene sulfide, and discloses a low-mold-temperature high-crystallization polyphenylene sulfide composite modified material as well as a preparation method and application thereof. The preparation method comprises the following steps: S1, uniformly stirring the filler, adding the coupling agent for crosslinking, and stirring again; s2, adding the compatilizer, the lubricant and the antioxidant, and uniformly stirring and mixing; s3, adding polyphenylene sulfide and polyethylene glycol terephthalate, and uniformly stirring; and S4, plasticizing, shearing and mixing to obtain the low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material. The low-mold-temperature high-crystallization polyphenylene sulfide composite modified material prepared by the method has the advantages that a high-crystallization modified polyphenylene sulfide product with the crystallization rate of 52-56% can be obtained under the mold temperature condition of 90-120 DEG C, and meanwhile, the appearance performance, the mechanical performance, the physical performance, the heat resistance, the cold resistance and the electrical performance of the modified material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyphenylene sulfide, in particular to a low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material and a preparation method and application thereof. Background Art

[0002] The polyphenylene sulfide material currently on the market is a special engineering plastic with high crystallinity. The main chain of its molecule is composed of alternating benzene rings and sulfur atoms. This structure gives polyphenylene sulfide PPS extremely high rigidity and crystallization ability.

[0003] However, under normal circumstances, when polyphenylene sulfide is molded at a relatively low mold temperature, its crystallinity will decrease. The crystallinity of the injection molded products obtained by polyphenylene sulfide at a low mold temperature (below 95°C) is only less than 15%; for example, under mold temperature conditions below 135°C, polyphenylene sulfide cannot produce an appropriate crystalline molecular structure, resulting in a low crystallinity of the injection molded parts, resulting in poor appearance and low performance of the parts. In addition, the high mold temperature (140-160°C) of the traditional process can achieve a high crystallinity of 50% to 65%, and all the performance of such parts can be met, but the steel requirements for the mold and the cost of mold processing are relatively high. In the later use of the mold, due to the need for high mold temperature, the cost of electricity, mold maintenance cost, and mold use cost are very high, and product quality control is very difficult.

[0004] In order to solve the above problems, technical engineers have adopted methods such as compounding polytetrafluoroethylene to solve this problem, but the cost of citing materials such as polytetrafluoroethylene is high and the material compatibility is low.

[0005] Therefore, how to develop a material with low cost, high compatibility and high crystallinity for the injection molded products is a problem that technicians need to solve at present. Summary of the invention

[0006] In order to overcome the problems existing in the related art, the present invention provides a low mold temperature and high crystallinity polyphenylene sulfide composite modified material;

[0007] Another object of the present invention is to provide a method for preparing a low mold temperature and high crystallinity polyphenylene sulfide composite modified material;

[0008] Another object of the present invention is to provide an application of a low mold temperature and high crystallization polyphenylene sulfide composite modified material;

[0009] Another object of the present invention is to provide an injection molded part.

[0010] A low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material is prepared from the following components in parts by weight:

[0011]

[0012] Preferably, the filler includes at least one of wollastonite, talc, barium sulfate, calcium sulfate and silicon carbide.

[0013] Preferably, the compatibilizer includes at least one of ethylene-acrylate-glycidyl methacrylate and a maleic anhydride grafted compatibilizer.

[0014] Preferably, the fiber includes at least one of glass fiber, carbon fiber, aramid fiber and basalt fiber.

[0015] Preferably, the coupling agent includes at least one of γ-glycidyloxypropyltrimethoxysilane and triisostearyl isopropyl titanate.

[0016] Preferably, the lubricant includes at least one of silicone powder and pentaerythritol stearate.

[0017] Preferably, the antioxidant includes at least one of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 2,6-di-tert-butyl-4-methylphenol.

[0018] A method for preparing the low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material comprises the following steps:

[0019] S1. Stir the filler evenly, add coupling agent for cross-linking, and stir again;

[0020] S2. Add compatibilizer, lubricant and antioxidant, and stir to mix evenly;

[0021] S3, adding polyphenylene sulfide and polyethylene terephthalate, and stirring evenly;

[0022] S4, after plasticizing, shearing and mixing, a low-mold-temperature and high-crystalline polyphenylene sulfide composite modified material is obtained.

[0023] Preferably, after the S4 is plasticized, sheared and mixed, it is kneaded, compressed and blended to obtain a low-mold-temperature and high-crystalline polyphenylene sulfide composite modified material.

[0024] Furthermore, after the plasticization, shearing and mixing in S4, the fiber is added, and then plasticization, shearing, dispersion, mixing and kneading, compression, and blending granulation are performed to obtain a low mold temperature and high crystallinity polyphenylene sulfide composite modified material.

[0025] Preferably, the fibers are added via a side feeder, and then plasticized, sheared by a screw block, dispersed, mixed and kneaded, compressed, and blended into granules to obtain a low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material.

[0026] Furthermore, in the step S1, the filler is stirred evenly at a stirring speed of 2500 to 3500 rpm and a stirring temperature of 105 to 115°C.

[0027] Furthermore, in the cross-linking by adding the coupling agent in S1, the cross-linking temperature is 120-130°C; in the stirring again in S1, the stirring speed is 800-1200 rpm, and the stirring temperature is 90-100°C.

[0028] Preferably, the crosslinking temperature is 125°C.

[0029] Preferably, the stirring time in S1 is 8 to 12 minutes.

[0030] Preferably, the stirring time in S1 is 10 minutes.

[0031] Preferably, the stirring speed during the stirring and mixing in S2 is 800 to 1200 rpm, and the stirring time is 4 to 8 minutes.

[0032] Preferably, the stirring time is 5 minutes.

[0033] Furthermore, the stirring speed of S3 is 2000-2500 rpm, and the stirring temperature is 110-115°C.

[0034] Preferably, the stirring time of S3 is 5 minutes.

[0035] Furthermore, the plasticizing temperature of S4 is 275-315°C.

[0036] Preferably, S4 is plasticized, sheared by the screw block, and mixed in a twin-screw extruder with a length-to-diameter ratio of 40:1 to the side feed port of the fifth section of the twin-screw extruder.

[0037] An application of the low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material is used for preparing injection molded parts.

[0038] An injection molded part is prepared from the low mold temperature and high crystallinity polyphenylene sulfide composite modified material.

[0039] Furthermore, the injection temperature during preparation is 285-300°C and the mold temperature is 90-120°C.

[0040] In order to obtain a polyphenylene sulfide (PPS) composite modified material with high crystallinity under low mold temperature conditions, the present invention adopts a copolymerization modification method of polyphenylene sulfide (PPS) and polyethylene terephthalate (PET), wherein: the melting heat enthalpy value of polyphenylene sulfide PPS when completely melted at 315°C is 77.5J / g, and its maximum crystallinity can reach 65%, and the melting heat enthalpy value of PET when completely melted at 255°C is 139-140J / g, and its crystallinity is completely completed. The polyethylene glycol (PEG) high molecular polymer in polyethylene terephthalate (PET) is used to form a liquid-liquid separation phase of polyphenylene sulfide (PPS) and polyethylene terephthalate (PET) materials during the melting process, and then each forms an island-shaped spherulite nucleus. The respective effects of the crystallization enthalpy of PET being greater than the melting enthalpy and the melting enthalpy of PPS being greater than the crystallization enthalpy are used. After PET and PPS complete their respective crystal nuclei, a compatibilizer is added to make them compatible.

[0041] There is a rigid benzene ring structure in the molecular chain of polyethylene terephthalate (PET) material, which makes its molecular chain have high rigidity. The main chain of polyphenylene sulfide PPS is composed of benzene rings and sulfur atoms arranged alternately. This structure makes polyphenylene sulfide PPS have very high rigidity and high crystallinity. The chemical structure of polyphenylene sulfide PPS contains repeating units of p-phenylene sulfide. In addition, it is highly symmetrical with the molecular chain of polyethylene terephthalate PET. These units are connected together by stable chemical bonds to form a highly regular crystal structure. Thereby, the nucleation and crystal growth rate of polyphenylene sulfide (pps) and polyethylene terephthalate (PET) are improved. At the same time, through the copolymerization of the two substances, the melting heat enthalpy of the copolymer is reduced and the crystallization enthalpy of the copolymer is increased. The copolymer can achieve high crystallization effect at low mold temperature.

[0042] In the preparation method of the present invention, the copolymer of each component is formed during the melting process, thereby increasing the speed of nucleation and crystal growth of polyphenylene sulfide (PPS). In addition, the molecular chains of polyphenylene sulfide (PPS) and polyethylene terephthalate (PET) are highly symmetrical, and this symmetry also gives the synergy of nucleation and crystal morphology during the crystallization process of the copolymer.

[0043] Specifically, polyethylene terephthalate (PET) needs to start to generate crystal nuclei at a plasticizing temperature of 80°C to 182°C, and polyphenylene sulfide (PPS) starts to generate crystal nuclei at a plasticizing temperature of 295°C to 315°C. This means that in different plasticizing temperature regions, the two materials respectively form liquid-liquid separation phases of plasticized substances, and there is a large difference in the temperature at which the crystal nuclei of the two materials are generated, thus forming an island structure of polyphenylene sulfide (PPS) and polyethylene terephthalate (PET) copolymer crystals. With the addition of a compatibilizer to make it compatible with various mixed substances, and the addition of a coupling agent to improve its intermolecular interface, the island structure of the crystals of the copolymer mainly composed of polyphenylene sulfide (PPS) and polyethylene terephthalate (PET) bridges each other to form continuous crystals. By adding different substances and different numbers of formula combinations, the modified granulation with various performance requirements required is completed by extrusion in a twin-screw extruder, and a low mold temperature and high crystallization polyphenylene sulfide composite modified material is prepared.

[0044] The beneficial effects of the technical solution of the present invention are:

[0045] The low-mold-temperature high-crystallization polyphenylene sulfide composite modified material prepared by the method of the present invention has the ability to obtain a modified polyphenylene sulfide product with high crystallization (crystallization rate of 52-56%) under a mold temperature of 90-120°C. At the same time, the appearance performance, mechanical properties, physical properties, heat resistance, cold resistance, electrical properties, etc. of the modified material are improved, and the injection molding industry can save mold steel costs, mold processing costs, injection molding costs, and mold life costs, and improve the quality of the product. The difficulties caused by mold problems, processing problems, quality problems, and cost problems in the use of modified polyphenylene sulfide materials in the injection molding industry are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.

[0047] Figure 1 This is a flow chart for preparing the low mold temperature and high crystallinity polyphenylene sulfide composite modified material of Example 1. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] 1. A low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material is prepared from the following components in parts by weight:

[0051]

[0052] 2. The method for preparing a low-mold-temperature high-crystallization polyphenylene sulfide composite modified material comprises the following steps (such as Figure 1 ):

[0053] S1, stir the filler evenly (stirring speed is 2500 rpm, stirring temperature is 105°C), add coupling agent for cross-linking (cross-linking temperature is 120°C), and stir again (stirring speed is 1000 rpm, stirring temperature is 95°C, stirring time is 10 minutes);

[0054] S2. After adding compatibilizer, lubricant and antioxidant, stir and mix evenly (stirring speed is 1000 rpm, stirring time is 5 minutes);

[0055] S3, adding polyphenylene sulfide and polyethylene terephthalate, stirring evenly (stirring speed is 2300 rpm, stirring temperature is 110° C.);

[0056] S4. Plasticizing (temperature of 300°C), thread block shearing, and mixing are carried out in a twin-screw extruder with a length-to-diameter ratio of 40:1 to the side feeding port of the twin-screw extruder; adding fibers through the side feeding machine, and then plasticizing, thread block shearing, dispersion, mixing and kneading, compression, and blending granulation are carried out to obtain a low-mold-temperature and high-crystalline polyphenylene sulfide composite modified material.

[0057] 3. Injection molded parts are prepared from low mold temperature and high crystallization polyphenylene sulfide composite modified materials. The injection temperature during preparation is 290°C and the mold temperature is 95°C.

[0058] 4. Carry out tests on crystallization rate, appearance performance, mechanical properties, physical properties, heat resistance, cold resistance, electrical properties, etc.

[0059] Example 2

[0060] 1. A low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material is prepared from the following components in parts by weight:

[0061]

[0062] 2. The method for preparing a low mold temperature and high crystallization polyphenylene sulfide composite modified material comprises the following steps:

[0063] S1. Stir the coupling agent evenly (stirring speed is 800 rpm, stirring temperature is 90°C, and stirring time is 8 minutes);

[0064] S2, after adding compatibilizer, lubricant and antioxidant, stir and mix evenly (stirring speed is 800 rpm, stirring time is 4 minutes);

[0065] S3, add polyphenylene sulfide and polyethylene terephthalate, and stir evenly (stirring speed is 2000 rpm, stirring temperature is 110° C., and stirring time is 5 minutes);

[0066] S4. Plasticizing (temperature of 275°C), thread block shearing, and mixing are carried out in a twin-screw extruder with a length-to-diameter ratio of 40:1 to the side feeding port of the twin-screw extruder; adding fibers through the side feeding machine, and then plasticizing, thread block shearing, dispersion, mixing and kneading, compression, and blending granulation are carried out to obtain a low-mold-temperature and high-crystalline polyphenylene sulfide composite modified material.

[0067] 3. Injection molded parts are prepared from low mold temperature and high crystallization polyphenylene sulfide composite modified materials. The injection temperature during preparation is 300°C and the mold temperature is 120°C.

[0068] 4. Carry out tests on crystallization rate, appearance performance, mechanical properties, physical properties, heat resistance, cold resistance, electrical properties, etc.

[0069] Example 3

[0070] 1. A low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material is prepared from the following components in parts by weight:

[0071]

[0072] 2. The method for preparing a low mold temperature and high crystallization polyphenylene sulfide composite modified material comprises the following steps:

[0073] S1, stir the filler evenly (stirring speed is 3500 rpm, stirring temperature is 115°C), add coupling agent for cross-linking (cross-linking temperature is 130°C), and stir again (stirring speed is 1200 rpm, stirring temperature is 100°C, stirring time is 12 minutes);

[0074] S2, after adding compatibilizer, lubricant and antioxidant, stir and mix evenly (stirring speed is 1200 rpm, stirring time is 8 minutes);

[0075] S3, adding polyphenylene sulfide and polyethylene terephthalate, stirring evenly (stirring speed is 2500 rpm, stirring temperature is 115°C);

[0076] S4. Plasticizing (temperature of 315°C), screw block shearing, dispersion, mixing and kneading, compression, and blending and granulation are carried out in a twin-screw extruder with a length-diameter ratio of 40:1 to obtain a low-mold-temperature and high-crystalline polyphenylene sulfide composite modified material.

[0077] 3. Injection molded parts are prepared from low mold temperature and high crystallization polyphenylene sulfide composite modified materials. The injection temperature during preparation is 285°C and the mold temperature is 90°C.

[0078] 4. Carry out tests on crystallization rate, appearance performance, mechanical properties, physical properties, heat resistance, cold resistance, electrical properties, etc.

[0079] Comparative Example 1

[0080] The technical solution of Comparative Example 1 is similar to that of Example 1, except that polyethylene terephthalate, filler and compatibilizer are not added, and the injection molding temperature is 290°C.

[0081] Comparative Example 2

[0082] The technical solution of Comparative Example 2 is similar to that of Example 1, except that the plasticizing temperature is 320°C.

[0083] Results Analysis

[0084] When polyethylene terephthalate (PET) resin is not added, the molecular chains of polyphenylene sulfide PPS resin begin to move and gradually soften during the plasticization process. When the polyphenylene sulfide PPS resin is melted, the temperature gradually drops and crystal nuclei begin to form. Because too low a temperature will inhibit the formation of crystal nuclei, the corresponding crystal nucleus formation temperature needs to be maintained during the molding process. After the crystal nuclei are formed, the PPS molecular chains begin to grow into crystals on these nuclei. The shape and size of the crystals depend on temperature and time. For example, in the range of 235-265℃, with the increase of isothermal crystallization temperature, the spherulite morphology changes from a small and partially bundled structure to a large and perfect structure, which means that polyphenylene sulfide PPS resin needs to be in a high mold temperature state to start crystallization. According to the principle that the melting enthalpy of polyphenylene sulfide PPS resin is greater than the crystallization enthalpy, the melting heat enthalpy value of polyphenylene sulfide PPS when it is completely melted at 315℃ is 77.5J / g, and its maximum crystallinity can reach 65%. According to differential scanning calorimetry (DSC), the crystallization rate of polyphenylene sulfide PPS resin can be guaranteed to be 45% when the mold temperature is in an isothermal state of 150℃, and the basic requirements for the use of polyphenylene sulfide PPS resin can be met in the use process. Despite this, the quality of the product, such as appearance performance, mechanical properties, physical properties, heat resistance, cold resistance, electrical properties, etc., will still be reduced, or because the mold needs a high mold temperature to ensure the molding of the product, the use of particularly good steel and the long-term production required electricity will increase the mold steel cost, mold processing cost, injection molding cost and mold life cost.

[0085] Comparing the properties of Table 2, in Comparative Example 1, since PET was not added and the injection molding temperature was low (290°C), the formation of crystal nuclei was inhibited, the molecular chain of PPS could not be fully crystallized, and the crystallization rate was only 15%. This significantly affected the performance of the material, making the key mechanical properties of Comparative Example 1 such as notched impact strength, tensile strength, flexural strength and flexural modulus significantly lower than those of Example 1. This low crystallinity also led to a decrease in the dimensional stability and heat resistance of the material, which ultimately manifested as poor appearance quality and electrical properties.

[0086] In contrast, PET resin is added in Example 1. The introduction of PET promotes the crystallization of PPS during the plasticization process of PPS through the benzene ring structure in its molecular chain, forming more and more stable crystal nuclei, so that the crystallization rate reaches 56%. This high crystallinity greatly improves the mechanical properties of the material, such as the notched impact strength from 8.5 J / m to 13 J / m, and the tensile strength from 145 MPa to 180 MPa. In addition, the addition of PET also improves the appearance of the material, giving it a mirror effect on the surface and eliminating the appearance of glass fiber grain.

[0087] For Comparative Example 2, the plasticizing temperature is increased to 320°C. Although this high temperature can promote rapid melting of the material, it causes thermal degradation of the PET and PPS molecular chains, reducing the overall performance of the material. Although its crystallization rate can still reach 50%, the structural instability caused by the high temperature causes the mechanical properties to be slightly lower than those of Example 1, especially the decrease in tensile strength and bending strength. In addition, too high a temperature may have a negative impact on the surface quality of the material. Although its appearance is still mirror-like, the overall quality is lower than that of Example 1.

[0088] Table 2 Performance test results

[0089] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Notched impact strength (J / m) 13 12 12 8.5 11 Tensile strength(MPa) 180 180 175 145 170 Elongation at break (%) 2.2 2.2 2.15 1.2 2.0 Bending strength(MPa) 280 278 275 240 270 Flexural modulus (MPa) 13500 13350 13300 8500 13285 <![CDATA[Density (g / cm 3 )]]> 1.65 1.645 1.63 1.61 1.62 Heat Deflection Temperature 265℃ 265℃ 265℃ 258℃ 263℃ Crystallization rate 56% 53% 52% 15% 50% Crystallization time 2 seconds 3 seconds 4 seconds 10 seconds 5 seconds Appearance Mirror Mirror Mirror Fiberglass Mirror Volume resistance Ω.m <![CDATA[10 16 ]]> <![CDATA[10 16 ]]> <![CDATA[10 16 ]]> <![CDATA[10 13 ]]> <![CDATA[10 16 ]]> Dielectric strength MV / mm 30 28 25 12 22

[0090] In addition, the low mold temperature and high crystallization polyphenylene sulfide composite modified material and its preparation method provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technicians in this field, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A low mold temperature and high crystallization polyphenylene sulfide composite modified material, characterized in that: The material is prepared from the following components in parts by weight:

2. A method for preparing the low mold temperature and high crystallinity polyphenylene sulfide composite modified material according to claim 1, characterized in that: The following steps are involved: S1. Stir the filler evenly, add coupling agent for cross-linking, and stir again; S2. Add compatibilizer, lubricant and antioxidant, and stir to mix evenly; S3, adding polyphenylene sulfide and polyethylene terephthalate, and stirring evenly; S4, after plasticizing, shearing and mixing, a low-mold-temperature and high-crystalline polyphenylene sulfide composite modified material is obtained.

3. The method for preparing the low mold temperature and high crystallinity polyphenylene sulfide composite modified material according to claim 2, characterized in that: After the plasticization, shearing and mixing in S4, the fibers are added, and plasticization, shearing, dispersion, mixing and kneading, compression, and blending and granulation are performed again to obtain a low mold temperature and high crystallinity polyphenylene sulfide composite modified material.

4. The method for preparing the low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material according to claim 2, characterized in that: In step S1, the filler is stirred uniformly at a speed of 2500 to 3500 rpm and a temperature of 105 to 115°C.

5. The method for preparing the low mold temperature and high crystallinity polyphenylene sulfide composite modified material according to claim 2, characterized in that: In the cross-linking by adding the coupling agent in S1, the cross-linking temperature is 120-130°C; in the stirring again in S1, the stirring speed is 800-1200 rpm and the stirring temperature is 90-100°C.

6. The method for preparing the low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material according to claim 2, characterized in that: The stirring speed of S3 is 2000-2500 rpm, and the stirring temperature is 110-115°C.

7. The method for preparing the low-mold-temperature and high-crystallization polyphenylene sulfide composite modified material according to claim 2, characterized in that: The plasticizing temperature in S4 is 275-315°C.

8. An application of the low mold temperature and high crystallinity polyphenylene sulfide composite modified material according to claim 1, characterized in that: Used to prepare injection molded parts.

9. An injection molded part, characterized in that: The polyphenylene sulfide composite modified material with low mold temperature and high crystallinity is prepared from the polyphenylene sulfide composite modified material according to claim 1.

10. The injection molded part according to claim 9, characterized in that: The injection temperature during preparation is 285-300°C and the mold temperature is 90-120°C.

Citation Information

Patent Citations

  • Polyphenylene sulfide / polyethylene terephthalate (PPS / PET) composite material and preparation method thereof

    CN101781460A

  • High-strength polyphenylene sulfide / polyethylene terephthalate blend resin composition and its preparation method

    CN102272230A

  • PET (polyethylene terephthalate) composite material and preparation method thereof

    CN103497490A

  • Polyphenylene sulfide composition and preparation method thereof

    CN106221218A

  • Polyphenylene sulfide resin composition, fiber and method for producing them

    JP2004231908A