High-temperature-resistant colored paint, colored coating carbon ceramic brake disc and preparation method of colored coating carbon ceramic brake disc

By applying high-temperature resistant colored paint on the carbon ceramic brake disc to form a variable color coating, the problem of determining wear of carbon ceramic brake discs is solved, safe and intuitive service life management is achieved, and the appearance of the brake disc is beautified.

CN118909502APending Publication Date: 2024-11-08福建康碳防务材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191627.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing carbon ceramic brake discs are difficult to determine wear conditions intuitively and safely, which affects service life management.

Method used

High-temperature resistant colored coatings, including base and top layer coatings, are coated on the surface of carbon ceramic brake discs, and a colored coating is formed through chemical vapor deposition and silicone permeation treatment. The brake disc life can be determined as the coating changes with the wear color.

Benefits of technology

Intuitively judge the brake disc wear through color changes, improving the safety and reliability of service life management, and beautifying the appearance of the brake disc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909502A_ABST
    Figure CN118909502A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon ceramic brake discs, and particularly relates to a high-temperature-resistant colored coating, a colored coating carbon ceramic brake disc and a preparation method of the colored coating carbon ceramic brake disc. The high-temperature-resistant colored coating provided by the invention comprises a prime coating and a surface coating which are independently subpackaged, the prime paint is prepared from 8.5 to 9.5 percent of carbon powder, 25 to 32 percent of silicon carbide powder, 9 to 12 percent of organic polymer, 3 to 5 percent of glycerol, 0.5 to 2 percent of polyether modified organic silicon and 46 to 49 percent of water; the surface layer coating comprises 10 to 12 percent of pigment, 25 to 30 percent of silicon carbide powder, 10 to 12 percent of organic polymer, 3 to 5 percent of glycerol, 0.5 to 2 percent of polyether modified organic silicon and 46 to 49 percent of water. According to the colored coating carbon ceramic brake disc prepared from the high-temperature-resistant colored paint provided by the invention, the wear condition of the carbon ceramic brake disc can be confirmed by checking the color change of the disc surface of the carbon ceramic brake disc, so that the high-temperature-resistant colored paint is more visual and safer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of carbon ceramic brake discs, and in particular relates to a high temperature resistant colored coating, a colored coated carbon ceramic brake disc and a preparation method thereof. Background Art

[0002] With the rapid development of the automobile market, people are paying more and more attention to the safety of automobile driving, which highlights the importance of automobile brake discs. Traditional brake discs are cast iron discs, which are characterized by poor wear resistance, high density, and large mass, which are not conducive to improving the braking performance of automobiles. Carbon ceramic brake discs have low loss and long life, and have strong mechanical properties. Especially when the car is driving on a steep slope or needs to brake frequently, ordinary cast iron discs are prone to soften and heat up, while carbon ceramic brake discs have more stable braking performance, which is why they are increasingly favored by people.

[0003] In order to meet the market's demand for high performance and high strength of automobiles, the requirements for brake discs are getting higher and higher. As the use time of the car increases, the brake disc surface will wear and become scrapped. However, it is difficult to define the wear and scrap of current carbon ceramic brake discs. The only way to judge the braking effect is through the driving process of the car, which lacks safety. Summary of the invention

[0004] The purpose of the present invention is to provide a high temperature resistant colored coating, a colored coated carbon ceramic brake disc and a preparation method thereof. The high temperature resistant colored coating for the carbon ceramic brake disc provided by the present invention can beautify the appearance of the carbon ceramic brake disc, and the wear condition can be confirmed by checking the color of the carbon ceramic brake disc surface.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a high temperature resistant colored coating for a carbon ceramic brake disc, comprising a bottom coating and a surface coating which are independently packaged;

[0007] The primer comprises the following components in percentage by mass: 8.5-9.5% carbon powder, 25-32% silicon carbide powder, 9-12% organic polymer, 3-5% glycerol, 0.5-2% polyether modified silicone and 46-49% water;

[0008] The surface coating comprises the following components in percentage by mass: 10-12% of colorant, 25-30% of silicon carbide powder, 10-12% of organic polymer, 3-5% of glycerol, 0.5-2% of polyether modified organic silicon and 46-49% of water.

[0009] Preferably, the mass ratio of the base coating to the surface coating is (1.2-1.25):1.

[0010] Preferably, the organic polymers in the primer and topcoat include polyacrylamide and / or polyvinyl alcohol.

[0011] Preferably, the colorant includes cobalt blue or vanadium zirconium yellow.

[0012] The present invention provides a method for preparing a colored coated carbon ceramic brake disc, comprising the following steps:

[0013] Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform;

[0014] Processing the C / C preform into a C / C brake disc;

[0015] After the surface of the C / C brake disc is coated with the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution, heat treatment is performed to obtain a semi-finished product, wherein the coating comprises the following steps: after the surface of the C / C brake disc is coated with the base coating of the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution, a first dehumidification treatment is performed, and then the surface coating of the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution is coated, and a second dehumidification treatment is performed;

[0016] The semi-finished product is subjected to siliconizing treatment to obtain the colored coated carbon ceramic brake disc.

[0017] Preferably, the method for preparing the needle-punched structural carbon fiber preform comprises the following steps:

[0018] The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns;

[0019] The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated blank, and the laminated blank is needle-punched to obtain a needle-punched structural carbon fiber preform; the thickness of the laminated blank is 18 to 30 mm; the density of the laminated blank is 0.58 to 0.63 g / m 3 The density of the acupuncture is 25 needles / cm 2 .

[0020] Preferably, the density of the C / C preform is ≥1.4 g / m 3 The reducing gas for the chemical vapor deposition is hydrogen, the flow rate of natural gas is 45-75 SLM, the flow rate of hydrogen is 25-50 SLM, the temperature of the chemical vapor deposition is 1000-1100°C, and the deposition time is 160h.

[0021] Preferably, the relative humidity of the first dehumidification treatment and the second dehumidification treatment is 30-40% RH, and the time is 8-12 hours;

[0022] The heat treatment temperature is 80° C. and the time is 3 hours.

[0023] Preferably, the siliconizing treatment is a molten siliconizing treatment, the temperature of the molten siliconizing treatment is 1350-1600° C., the holding time is 1-3 hours, and the molten siliconizing treatment is carried out under vacuum conditions.

[0024] The present invention provides a colored coated carbon ceramic brake disc prepared by the preparation method described in the above technical solution.

[0025] The invention provides a high temperature resistant colored coating for a carbon ceramic brake disc, comprising a bottom coating and a surface coating which are independently packaged; the bottom coating comprises the following components in percentage by mass: 8.5-9.5% carbon powder, 25-32% silicon carbide powder, 9-12% organic polymer, 3-5% propylene glycol, 0.5-2% polyether modified silicone and 46-49% water; the surface coating comprises the following components in percentage by mass: 10-12% colorant, 25-30% silicon carbide powder, 10-12% organic polymer, 3-5% propylene glycol, 0.5-2% polyether modified silicone and 46-49% water. The high temperature resistant colored coating provided by the invention has the characteristic of high temperature resistance, and when applied to the preparation of the colored coating of the carbon ceramic brake disc, it can not only beautify the appearance of the carbon ceramic brake disc, but also the obtained colored coating carbon ceramic brake disc can confirm the wear of the carbon ceramic brake disc by checking the color change of the disc surface of the carbon ceramic brake disc, which is more intuitive and safe.

[0026] The invention provides a method for preparing a colored coated carbon-ceramic brake disc, comprising the following steps: using natural gas as a carbon source gas, and adopting a chemical vapor deposition method to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform; processing the C / C preform into a C / C brake disc; coating the surface of the C / C brake disc with the high-temperature resistant colored coating for the carbon-ceramic brake disc described in the above technical solution, and then performing heat treatment to obtain a semi-finished product, wherein the coating comprises the following steps: coating the surface of the C / C brake disc with a base coating of the high-temperature resistant colored coating for the carbon-ceramic brake disc described in the above technical solution, and then performing a first dehumidification treatment, and then coating the surface coating of the high-temperature resistant colored coating for the carbon-ceramic brake disc described in the above technical solution, and then performing a second dehumidification treatment; performing siliconization treatment on the semi-finished product to obtain the colored coated carbon-ceramic brake disc. In the preparation of the carbon-ceramic brake disc of the present invention, before the siliconizing treatment, the carbon-ceramic brake disc described in the above technical solution is coated on the surface of the C / C brake disc with a high temperature resistant colored coating, and subjected to dehumidification treatment and heat treatment, so that the obtained carbon-ceramic brake disc has a colored coating. During the braking process of the automobile, the coating is worn away. When the colored coating is completely worn away (the color disappears), it can be determined that the service life of the brake disc has ended. At the same time, the coating surface of the carbon-ceramic brake disc prepared by the present invention has color and is ornamental, which can meet the needs of some customers. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a physical picture of the colored coated carbon ceramic brake disc prepared in Example 1 of the present invention;

[0028] Figure 2 This is a photo of the colored coating on the surface of the colored coating carbon ceramic brake disc prepared in Example 1 of the present invention after all the colored coating has been worn away. DETAILED DESCRIPTION

[0029] The present invention provides a high temperature resistant colored coating for a carbon ceramic brake disc, comprising a bottom coating and a surface coating which are independently packaged;

[0030] The primer comprises the following components in percentage by mass: 8.5-9.5% carbon powder, 25-32% silicon carbide powder, 9-12% organic polymer, 3-5% glycerol, 0.5-2% polyether modified silicone and 46-49% water;

[0031] The surface coating comprises the following components in percentage by mass: 10-12% of colorant, 25-30% of silicon carbide powder, 10-12% of organic polymer, 3-5% of glycerol, 0.5-2% of polyether modified organic silicon and 46-49% of water.

[0032] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0033] The high temperature resistant colored coating for carbon ceramic brake disc provided by the present invention includes a primer that is packaged independently. In the present invention, the primer includes the following components in percentage by mass: 8.5-9.5% carbon powder, 25-32% silicon carbide powder, 9-12% organic polymer, 3-5% propylene glycol, 0.5-2% polyether modified silicone and 46-49% water. In terms of percentage by mass, the primer provided by the present invention includes 8.5-9.5% carbon powder, preferably 8.8-9.2%. In the present invention, the role of the carbon powder in the primer is that the carbon powder can react with the silicon material to form silicon carbide in the subsequent siliconization stage. In terms of percentage by mass, the primer provided by the present invention includes 25-32% silicon carbide powder, preferably 28-30%. In the present invention, the role of the silicon carbide powder in the primer is that the silicon carbide powder is the main component of the coating, constructs the matrix, and enhances the strength of the coating. In terms of percentage by mass, the primer provided by the present invention includes 9-12% organic polymer, preferably 10-11%. The organic polymer in the primer preferably includes polyacrylamide (PAM) and / or polyvinyl alcohol (PVA). In the present invention, the organic polymer in the primer has a bonding effect to enhance the viscosity between the materials. In terms of mass percentage, the primer provided by the present invention includes 3-5% glycerol, preferably 3.5-4.5%. In the present invention, the role of glycerol in the primer is that glycerol plays a softening role, prevents cracking, and moisturizes and prevents rapid loss of water. In terms of mass percentage, the primer provided by the present invention includes 0.5-2% polyether-modified silicone, preferably 1-1.5%. In the present invention, the role of the polyether-modified silicone in the primer is to reduce surface tension and eliminate bubbles in the glue. In a specific embodiment of the present invention, the polyether-modified silicone in the primer is preferably purchased from Dongguan Airui Chemical, and the product model is 608. In terms of mass percentage, the primer provided by the present invention includes 46-49% water, preferably 47-48%.

[0034] The high temperature resistant colored coating for carbon ceramic brake disc provided by the present invention includes a surface coating that is packaged independently. In the present invention, the surface coating includes the following components in percentage by mass: 10-12% colorant, 25-30% silicon carbide powder, 10-12% organic polymer, 3-5% propylene glycol, 0.5-2% polyether modified silicone and 46-49% water. In terms of percentage by mass, the surface coating provided by the present invention includes 10-12% colorant, preferably 10.5-11.5%. In the present invention, the colorant preferably includes cobalt blue or vanadium zirconium yellow. . In terms of percentage by mass, the surface coating provided by the present invention includes 25-30% silicon carbide powder, preferably 26-28%. In the present invention, the role of silicon carbide powder in the surface coating is that silicon carbide powder is the main component of the coating, constructs the matrix, and enhances the strength of the coating. In terms of percentage by mass, the surface coating provided by the present invention includes 10-12% organic polymer, preferably 10.5-11.5%. The organic polymer in the surface coating preferably includes polyacrylamide (PAM) and / or polyvinyl alcohol (PVA). In the present invention, the organic polymer in the surface coating has a bonding effect to enhance the viscosity between the materials. In terms of mass percentage, the surface coating provided by the present invention includes 3-5% glycerol, preferably 3.5-4.5%. In the present invention, the role of glycerol in the surface coating is that glycerol plays a softening role to prevent cracking, while moisturizing and preventing rapid loss of water. ,. In terms of mass percentage, the surface coating provided by the present invention includes 0.5-2% polyether-modified silicone, preferably 1-1.5%. In the present invention, the role of the polyether-modified silicone in the surface coating is to reduce surface tension and eliminate bubbles in the glue. In a specific embodiment of the present invention, the polyether-modified silicone in the surface coating is preferably purchased from Dongguan Airui Chemical, and the product model is 608. In terms of mass percentage, the surface coating provided by the present invention includes 46-49% water, preferably 47-48%.

[0035] In the present invention, the mass ratio of the base coating to the top coating is preferably (1.2-1.25):1.

[0036] When the high temperature resistant colored coating for carbon-ceramic brake discs provided by the present invention is used to prepare the coating of carbon-ceramic brake discs, the appearance of the brake discs can be beautified by adding the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution into the carbon-ceramic brake disc coating, and the wear condition can be confirmed by checking the color of the disc surface. After the colored coating is completely worn out (the color disappears), it can be determined that the service life of the brake disc has ended.

[0037] The present invention provides a method for preparing a high temperature resistant colored coating for a carbon ceramic brake disc according to the above technical solution. The method for preparing the primer preferably comprises the following steps: first mixing an organic polymer and water in the primer to obtain an organic polymer solution; second mixing the organic polymer solution and silicon carbide powder to obtain a second mixture; third mixing the first mixture, carbon powder, glycerol and polyether modified silicone to obtain the primer. In the present invention, the first mixing is preferably carried out in a mixer. When the organic polymer in the primer is preferably PAM, the temperature of the first mixing is preferably 40°C. When the organic polymer in the primer is preferably PVA, the temperature of the first mixing is preferably 90°C. The first mixing is preferably carried out under stirring. The stirring speed during the premixing is preferably 1000RPM. The obtained organic polymer solution is preferably a mixed uniform solution without visible particles. The temperature of the second mixing is preferably 40°C or 90°C. The time of the second mixing is preferably 3 to 5h. The second mixing is preferably carried out under stirring. The temperature of the third mixing is preferably 40°C or 90°C. The time of the third mixing is preferably 6 to 10 hours, and the third mixing is preferably carried out under stirring. The preparation method of the surface coating preferably includes the following steps: the organic polymer in the surface coating is mixed with water for the fourth time to obtain an organic polymer solution; the organic polymer solution and silicon carbide powder are mixed for the fifth time to obtain a fifth mixture; the fifth mixture, colorant, glycerol and polyether-modified silicone are mixed for the sixth time to obtain the surface coating. In the present invention, the fourth mixing is preferably carried out in a mixer, when the organic polymer in the surface coating is preferably PAM, the temperature of the fourth mixing is preferably 40°C, and when the organic polymer in the surface coating is preferably PVA, the temperature of the fourth mixing is preferably 90°C. The fourth mixing is preferably carried out under stirring, and the stirring speed during the premixing is preferably 1000RPM, and the obtained organic polymer solution is preferably a mixed uniform solution without visible particles. The temperature of the fifth mixing is preferably 40°C or 90°C. The time of the fifth mixing is preferably 3 to 5 hours, and the fifth mixing is preferably carried out under stirring. The temperature of the sixth mixing is preferably 40°C or 90°C. The sixth mixing is preferably performed for 6 to 10 hours, and is preferably performed under stirring.

[0038] The present invention provides a method for preparing a carbon ceramic brake disc with a colored coating, comprising the following steps:

[0039] Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform;

[0040] Processing the C / C preform into a C / C brake disc;

[0041] After the surface of the C / C brake disc is coated with the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution, heat treatment is performed to obtain a semi-finished product, wherein the coating comprises the following steps: after the surface of the C / C brake disc is coated with the base coating of the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution, a first dehumidification treatment is performed, and then the surface coating of the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution is coated, and a second dehumidification treatment is performed;

[0042] The semi-finished product is subjected to siliconizing treatment to obtain the colored coated carbon ceramic brake disc.

[0043] The invention uses natural gas as a carbon source gas and adopts a chemical vapor deposition method to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform.

[0044] In the present invention, the method for preparing the needle-punched structural carbon fiber preform preferably comprises the following steps:

[0045] The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns;

[0046] The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated blank, and the laminated blank is needle-punched to obtain a needle-punched structural carbon fiber preform; the thickness of the laminated blank is 18 to 30 mm; the density of the laminated blank is 0.58 to 0.63 g / m 3 The density of the acupuncture is 25 needles / cm 2 .

[0047] The present invention uses short-cut carbon fiber filaments to prepare the mesh tire, and uses long carbon fiber filaments to prepare the non-woven fabric. In the present invention, the short-cut carbon fiber filaments are preferably short-cut T400-24K carbon fiber filaments. The present invention has no special requirements for the specific preparation method of the mesh tire. The surface density of the mesh tire is preferably 160g / cm 2 The long carbon fiber yarn is preferably T400-24K carbon fiber yarn. The present invention has no special requirements on the specific preparation method of the non-woven fabric. The surface density of the non-woven fabric is preferably 360g / cm 2 .

[0048] After obtaining the mesh tire and the non-woven fabric, the present invention lays the mesh tire and the non-woven fabric in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated blank, and needle-punches the laminated blank to obtain a needle-punched structural carbon fiber preform; the thickness of the laminated blank is 18 to 30 mm; the density of the laminated blank is 0.58 to 0.63 g / m 3 The density of the acupuncture is 25 needles / cm2 In the present invention, when laying, the non-woven fabric is preferably used alternately in three directions of 0°, 60° and 90°. The thickness of the laminated body is preferably 18 to 30 mm, more preferably 20 to 25 mm. The density of the laminated body is preferably 0.58 to 0.63 g / m 3 , more preferably 0.59 to 0.61 g / m 3 .

[0049] The present invention uses natural gas as a carbon source gas and adopts a chemical vapor deposition (CVD) method to perform carbon densification on the needle-punched carbon fiber preform to obtain a C / C preform.

[0050] In the present invention, the deposition temperature of the chemical vapor deposition is preferably 1000-1100°C, the natural gas flow rate is preferably 45-75SLM, more preferably 48-70SLM, and further preferably 50-65SLM. The auxiliary gas is preferably ethane, and the flow rate of the auxiliary gas is preferably 20-35SLM. The reducing gas is preferably hydrogen, and the flow rate of hydrogen is preferably 25-50SLM, and more preferably 30-45SLM. The deposition time is preferably 160h. In the present invention, the density of the obtained C / C preform is preferably ≥1.4g / cm 3 .

[0051] After obtaining the C / C preform, the present invention processes the C / C preform into a C / C brake disc. The present invention has no special requirements on the specific implementation of the processing. The shape of the C / C brake disc is preferably annular.

[0052] After obtaining the C / C brake disc, the present invention applies the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution to the surface of the C / C brake disc and then performs heat treatment to obtain a semi-finished product, wherein the coating comprises the following steps: applying the bottom coating of the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution to the surface of the C / C brake disc and then performing a first dehumidification treatment, and then applying the top coating of the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution and then performing a second dehumidification treatment. The present invention preferably applies the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution to one of the surfaces of the C / C brake disc and then performs heat treatment; then applies the high temperature resistant colored coating for carbon-ceramic brake discs described in the above technical solution to the other surface of the C / C brake disc and then performs heat treatment to finally obtain a semi-finished product. The present invention has the same operating parameters for coating the high temperature resistant colored coating for carbon-ceramic brake discs and heat treatment on both surfaces of the C / C brake disc. In the present invention, when the high temperature resistant colored coating for carbon ceramic brake discs described in the above technical solution is applied to any surface of the C / C brake disc, the coating preferably includes the following steps: after applying the base coating of the high temperature resistant colored coating for carbon ceramic brake discs described in the above technical solution to the surface of the C / C brake disc, a first dehumidification treatment is performed, and then the surface coating of the high temperature resistant colored coating for carbon ceramic brake discs described in the above technical solution is applied, and then a second dehumidification treatment is performed. The specific coating method of the base coating is preferably spraying. The specific coating method of the surface coating is preferably spraying. The coating thickness of the surface coating is preferably 0.7 to 0.8 mm. The first dehumidification treatment preferably places the C / C brake disc coated with the base coating in an indoor environment, and uses dehumidification to perform the first dehumidification, the relative humidity of the first dehumidification (relative humidity of the indoor environment) is preferably 30 to 40% RH, and the time of the first dehumidification is preferably 8 to 12 hours. The second dehumidification treatment preferably places the C / C brake disc coated with the surface coating in an indoor environment and uses dehumidification to perform the second dehumidification. The relative humidity of the second dehumidification (relative humidity of the indoor environment) is preferably 30-40% RH, and the time of the second dehumidification is preferably 8-12 hours.

[0053] In the present invention, after coating a primer, a first dehumidification treatment, a surface coating, and a second dehumidification treatment are sequentially applied to any surface of the C / C brake disc, the sample subjected to the second dehumidification treatment is subjected to the heat treatment. The temperature of the heat treatment is preferably 80°C and the time is 3h. The heat treatment is preferably carried out in an oven. In the present invention, after coating a primer, a first dehumidification treatment, a surface coating, a second dehumidification treatment, and a heat treatment are sequentially applied to any surface of the C / C brake disc, the present invention preferably performs surface grinding on the heat-treated product, and the surface grinding is preferably carried out in a machining workshop. In the present invention, the surface after the heat treatment is preferably ground flat by the grinding.

[0054] After obtaining the semi-finished product, the present invention preferably performs a molding process on the semi-finished product before performing the siliconizing treatment. The molding process preferably includes: opening ventilation grooves on the semi-finished product. The molding process is preferably performed in a machining center.

[0055] After the forming process, the present invention performs siliconizing treatment on the semi-finished product after the forming process to obtain the carbon ceramic brake disc with the colored coating. In the present invention, the raw material used for the siliconizing treatment is preferably silicon powder, and the siliconizing treatment is preferably carried out in a siliconizing furnace. The present invention preferably places the silicon powder in a crucible with BN coated on the surface, and then places the semi-finished product on the silicon powder, and then places it in a siliconizing furnace for siliconizing treatment. In the present invention, the siliconizing treatment is preferably a molten siliconizing treatment, and the temperature of the molten siliconizing treatment is preferably 1350-1600°C, more preferably 1400-1550°C, the holding time is preferably 1-3h, and the heating time from room temperature to the temperature of the siliconizing treatment is preferably 25-30h. The molten siliconizing treatment is carried out under vacuum conditions. The present invention preferably raises the temperature of the siliconizing furnace from room temperature to 800°C.

[0056] In the present invention, after the siliconizing treatment, the present invention preferably performs surface grinding on the siliconized brake disc to obtain the carbon ceramic brake disc with the colored coating. In the present invention, the surface grinding is preferably performed in a machining workshop. The present invention preferably performs surface grinding on the siliconized brake disc to remove excess silicon material on the surface, and grinds until ceramic cracks appear.

[0057] The present invention provides a carbon-ceramic brake disc with a colored coating prepared by the preparation method described in the above technical solution.

[0058] The coating of the carbon ceramic brake disc with colored coating provided by the present invention has a special color. During the braking process of the automobile, the coating is worn away. When the colored coating is completely worn away (the color disappears), it can be determined that the service life of the brake disc has ended.

[0059] The coating surface of the colored-coated carbon-ceramic brake disc provided by the present invention has a special color and is ornamental, thereby meeting the needs of some customers.

[0060] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0061] Example 1

[0062] This embodiment provides a high temperature resistant colored coating for a carbon ceramic brake disc, including a base coating and a surface coating that are separately packaged;

[0063] The primer comprises the following components in percentage by mass: 9% carbon powder, 30% silicon carbide powder, 10% PAM, 4% glycerol, 1% polyether-modified silicone and 46% water;

[0064] The surface coating comprises the following components in percentage by mass: 12% of cobalt blue, 30% of silicon carbide powder, 10% of PAM, 4% of glycerol, 1% of polyether-modified organic silicon and 43% of water.

[0065] The method for preparing the high temperature resistant colored coating for carbon ceramic brake disc provided in this embodiment comprises the following steps:

[0066] The preparation method of the base coating is as follows: each raw material is weighed according to the weight, and then the weighed PAM and water are added to the mixer, and the heating (40°C) and stirring (1000rpm) are continuously turned on. After the PAM solution obtained by stirring is mixed evenly (no visible particles), silicon carbide powder is poured into the mixer, heated and stirred for 5 hours, and then carbon powder, polyether-modified silicone, and propylene glycol are added and stirred for 10 hours to obtain the base coating.

[0067] The preparation method of the surface coating is as follows: each raw material is weighed according to the weight, and then the weighed PAM and water are added to the mixer, and the heating (40°C) and stirring (1000rpm) are continuously turned on. After the PAM solution obtained by stirring is mixed evenly (no visible particles), silicon carbide powder is poured into the mixer, heated and stirred for 5 hours, and then cobalt blue, polyether-modified silicone and propylene glycol are added and stirred for 10 hours to obtain the surface coating.

[0068] This embodiment provides a method for preparing a colored coated carbon ceramic brake disc, comprising the following steps:

[0069] (1) Preparation of C / C brake discs. A non-woven fabric was prepared using 60 cm long T400-24K carbon fiber yarns, and a mesh was prepared using 6-7 cm long chopped T400-24K carbon fiber yarns. A cyclic laying method of one layer of mesh and one layer of non-woven fabric was adopted, wherein the non-woven fabric was used alternately at 0°, 60° and 90°, with a laying thickness of 30 mm and a volume density of 0.58-0.63 g / cm 3 Finally, acupuncture was performed with a density of 25 needles / cm 2 , forming a needle-punched carbon fiber preform. The needle-punched carbon fiber preform is then treated with chemical vapor deposition (CVI) at a deposition temperature of 1100°C and a deposition time of 160 hours. The deposition gases are natural gas and hydrogen, with a natural gas flow rate of 75 SLM and a hydrogen flow rate of 50 SLM. The density of the C / C preform reaches 1.4 g / cm 3 The C / C preform with the density reaching the standard after deposition is then processed into a ring-shaped C / C brake disc.

[0070] (2) Spraying. Surface A of a circular C / C brake disc: Pour the primer into a spray can and spray it onto the C / C brake disc using a spray device.

[0071] (3) Dehumidification. Place the sprayed C / C brake disc indoors, turn on the dehumidifier, set the humidity to 30-40% RH, and set the time to 12 hours.

[0072] (4) Spraying. Surface A of a ring-shaped C / C brake disc: Pour the surface coating into a spray can and then spray it onto the coating surface after dehumidification in step (3) using a spray device.

[0073] (5) Dehumidification. The steps are the same as step (3).

[0074] (6) Baking: The C / C brake disc after dehumidification in step (5) is transferred to an oven for baking at 80° C. for 3 h.

[0075] (7) Machining: The C / C brake disc baked in (6) is transferred to a machining workshop for surface turning of the coating to make the surface smooth.

[0076] (8) Spray the B surface of the annular C / C brake disc. The steps are the same as steps (2) to (7).

[0077] (9) Forming processing. The disc body after turning in (8) is transferred to a machining center for a series of forming processing such as opening ventilation grooves to obtain a semi-finished product.

[0078] (10) Siliconizing. Place silicon powder in a crucible coated with BN, place the C / C brake disc semi-finished product to be siliconized in step (9) on the silicon powder, and then transfer the crucible to a siliconizing furnace for melt siliconizing treatment, wherein the maximum temperature of the melt siliconizing treatment is 1550°C, the heating time from room temperature to the maximum temperature of the melt siliconizing treatment is 30 hours, and the maximum temperature holding time is 3 hours. During the heating process, when the room temperature reaches 800°C, nitrogen is filled into the siliconizing furnace, and the nitrogen pressure is 85 kPa.

[0079] (11) Finishing: The brake disc after siliconizing in step (10) is transferred to a machining workshop for surface grinding to remove excess silicon material on the surface, and is ground until ceramic cracks appear.

[0080] The actual picture of the carbon ceramic brake disc with colored coating prepared in this embodiment is as follows Figure 1 shown.

[0081] Figure 2 This is a photo of the carbon ceramic brake disc with colored coating prepared in this embodiment after service, with the colored coating on the surface completely worn out.

[0082] Example 2

[0083] This embodiment provides a high temperature resistant colored coating for a carbon ceramic brake disc, including a base coating and a surface coating that are separately packaged;

[0084] The primer comprises the following components in percentage by mass: 9% carbon powder, 28% silicon carbide powder, 10% PVA, 3% glycerol, 1% polyether-modified silicone and 49% water;

[0085] The surface coating comprises the following components in percentage by mass: 10% cobalt blue, 28% silicon carbide powder, 10% PVA, 3% glycerol, 1% polyether modified organic silicon and 48% water.

[0086] The method for preparing the high temperature resistant colored coating for carbon ceramic brake disc provided in this embodiment comprises the following steps:

[0087] The preparation method of the base coating is as follows: each raw material is weighed according to the weight, and then the weighed PAM and water are added to the mixer, and the heating (40°C) and stirring (1000rpm) are continuously turned on. After the PAM solution obtained by stirring is mixed evenly (no visible particles), silicon carbide powder is poured into the mixer, heated and stirred for 5 hours, and then carbon powder, polyether-modified silicone, and propylene glycol are added and stirred for 10 hours to obtain the base coating.

[0088] The preparation method of the surface coating is as follows: each raw material is weighed according to the weight, and then the weighed PAM and water are added to the mixer, and the heating (40°C) and stirring (1000rpm) are continuously turned on. After the PAM solution obtained by stirring is mixed evenly (no visible particles), silicon carbide powder is poured into the mixer, heated and stirred for 5 hours, and then cobalt blue, polyether-modified silicone and propylene glycol are added and stirred for 10 hours to obtain the surface coating.

[0089] This embodiment provides a method for preparing a colored coated carbon ceramic brake disc, comprising the following steps:

[0090] (1) Preparation of C / C brake discs. A non-woven fabric was prepared using 60 cm long T400-24K carbon fiber yarns, and a mesh was prepared using 6-7 cm long chopped T400-24K carbon fiber yarns. A cyclic laying method of one layer of mesh and one layer of non-woven fabric was adopted, wherein the non-woven fabric was used alternately at 0°, 60° and 90°, with a laying thickness of 30 mm and a volume density of 0.58-0.63 g / cm 3 Finally, acupuncture was performed with a density of 25 needles / cm 2, forming a needle-punched carbon fiber preform. The needle-punched carbon fiber preform is then treated with chemical vapor deposition (CVI) at a deposition temperature of 1100°C and a deposition time of 160 hours. The deposition gases are natural gas and hydrogen, with a natural gas flow rate of 75 SLM and a hydrogen flow rate of 50 SLM. The density of the C / C preform reaches 1.4 g / cm 3 The C / C preform with the density reaching the standard after deposition is then processed into a ring-shaped C / C brake disc.

[0091] (2) Spraying. Surface A of a circular C / C brake disc: Pour the primer into a spray can and spray it onto the C / C brake disc using a spray device.

[0092] (3) Dehumidification. Place the sprayed C / C brake disc indoors, turn on the dehumidifier, set the humidity to 30-40% RH, and set the time to 12 hours.

[0093] (4) Spraying. Surface A of a ring-shaped C / C brake disc: Pour the surface coating into a spray can and then spray it onto the coating surface after dehumidification in step (3) using a spray device.

[0094] (5) Dehumidification. The steps are the same as step (3).

[0095] (6) Baking: The C / C brake disc after dehumidification in step (5) is transferred to an oven for baking at 80° C. for 3 h.

[0096] (7) Machining: The C / C brake disc baked in (6) is transferred to a machining workshop for surface turning of the coating to make the surface smooth.

[0097] (8) Spray the B surface of the annular C / C brake disc. The steps are the same as steps (2) to (7).

[0098] (9) Forming processing. The disc body after turning in (8) is transferred to a machining center for a series of forming processing such as opening ventilation grooves to obtain a semi-finished product.

[0099] (10) Siliconizing. Place silicon powder in a crucible coated with BN, place the C / C brake disc semi-finished product to be siliconized in step (9) on the silicon powder, and then transfer the crucible to a siliconizing furnace for melt siliconizing treatment, wherein the maximum temperature of the melt siliconizing treatment is 1550°C, the heating time from room temperature to the maximum temperature of the melt siliconizing treatment is 30 hours, and the maximum temperature holding time is 3 hours. During the heating process, when the room temperature reaches 800°C, nitrogen is filled into the siliconizing furnace, and the nitrogen pressure is 85 kPa.

[0100] (11) Finishing: The brake disc after siliconizing in step (10) is transferred to a machining workshop for surface grinding to remove excess silicon material on the surface, and is ground until ceramic cracks appear.

[0101] From the above embodiments, it can be seen that the carbon-ceramic brake disc with colored coating provided by the present invention has the following advantages compared with cast iron brake discs or carbon-ceramic brake discs with ordinary coatings: the coating of the carbon-ceramic brake disc with colored coating provided by the present invention has a special color, and during the braking process of the vehicle, the coating wears away. After the colored coating is completely worn away (the color disappears), it can be determined that the service life of the brake disc has ended.

[0102] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A high temperature resistant colored coating for a carbon ceramic brake disc, characterized in that: Includes independently packaged base coat and top coat; The primer comprises the following components in percentage by mass: 8.5-9.5% carbon powder, 25-32% silicon carbide powder, 9-12% organic polymer, 3-5% glycerol, 0.5-2% polyether modified silicone and 46-49% water; The surface coating comprises the following components in percentage by mass: 10-12% of colorant, 25-30% of silicon carbide powder, 10-12% of organic polymer, 3-5% of glycerol, 0.5-2% of polyether modified organic silicon and 46-49% of water.

2. The high temperature resistant colored coating for carbon ceramic brake disc according to claim 1, characterized in that: The mass ratio of the base coating to the surface coating is (1.2-1.25):

1.

3. The high temperature resistant colored coating for carbon ceramic brake disc according to claim 1 or 2, characterized in that: The organic polymers in the base coating and the top coating include polyacrylamide and / or polyvinyl alcohol.

4. The high temperature resistant colored coating for carbon ceramic brake disc according to claim 1 or 2, characterized in that: The colorant includes cobalt blue or vanadium zirconium yellow.

5. A method for preparing a colored coated carbon ceramic brake disc, characterized in that: The following steps are involved: Using natural gas as a carbon source gas, a chemical vapor deposition method is used to perform carbon densification on a needle-punched carbon fiber preform to obtain a C / C preform; Processing the C / C preform into a C / C brake disc; After coating the surface of the C / C brake disc with the high temperature resistant colored coating for carbon-ceramic brake discs as claimed in any one of claims 1 to 4, heat treatment is performed to obtain a semi-finished product, wherein the coating comprises the following steps: coating the surface of the C / C brake disc with the base coating of the high temperature resistant colored coating for carbon-ceramic brake discs as claimed in any one of claims 1 to 4, performing a first dehumidification treatment, and then coating the surface coating of the high temperature resistant colored coating for carbon-ceramic brake discs as claimed in any one of claims 1 to 4, performing a second dehumidification treatment; The semi-finished product is subjected to siliconizing treatment to obtain the colored coated carbon ceramic brake disc.

6. The preparation method according to claim 5, characterized in that: The method for preparing the needle-punched structural carbon fiber preform comprises the following steps: The mesh tire is prepared by using short-cut carbon fiber yarns, and the non-woven fabric is prepared by using long carbon fiber yarns; The mesh tire and the non-woven fabric are laid in a cyclic layering manner of one layer of mesh tire and one layer of non-woven fabric to obtain a laminated blank, and the laminated blank is needle-punched to obtain a needle-punched structural carbon fiber preform; the thickness of the laminated blank is 18 to 30 mm; the density of the laminated blank is 0.58 to 0.63 g / m 3 The density of the acupuncture is 25 needles / cm 2 .

7. The preparation method according to claim 5, characterized in that: The density of the C / C preform is ≥1.4 g / m 3 The reducing gas for the chemical vapor deposition is hydrogen, the flow rate of natural gas is 45-75 SLM, the flow rate of hydrogen is 25-50 SLM, the temperature of the chemical vapor deposition is 1000-1100°C, and the deposition time is 160h.

8. The preparation method according to claim 5, characterized in that: The relative humidity of the first dehumidification process and the second dehumidification process is 30-40% RH, and the time is 8-12 hours; The heat treatment temperature is 80° C. and the time is 3 hours.

9. The preparation method according to claim 5, characterized in that: The siliconizing treatment is a molten siliconizing treatment, the temperature of the molten siliconizing treatment is 1350-1600° C., the heat preservation time is 1-3 hours, and the molten siliconizing treatment is carried out under vacuum conditions.