Cellulose modified polyester polyurethane-polyacrylate aqueous dispersion for automobile water-based finish paint and preparation method of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion

By combining acetobutyl cellulose and polyester polyurethane prepolymer, cellulose modified polyester polyurethane-polyacrylate aqueous dispersion is prepared, which solves the insufficient leveling of automotive water-based topcoats and the matching of solvent-based cover paints. The problem of this has achieved improvements in the leveling property and mechanical properties of the coating.

CN118909503AActive Publication Date: 2024-11-08CHANGZHOU WUJIN CHENGUANG METALLIC COATING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411211872.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The leveling property of existing automotive water-based topcoats and the matching properties of solvent-based hood paints result in uneven surfaces and poor orientation effects, and the existing cellulose-modified polyester polyurethane aqueous dispersions cannot effectively solve these problems. question.

Method used

Cellulose modified polyester polyurethane is prepared by dissolving acetobutyl cellulose in N-methylpyrrolidone and combining with polyester polyurethane prepolymer. By adding acrylic monomers and initiators, the reaction conditions and neutralizing agent are controlled to prepare cellulose modified polyester polyurethane. - Polyacrylate aqueous dispersion, realize molecular interpenetration and emulsification of acetobutan cellulose and polymer chains, and improve the leveling and mechanical properties of the coating.

Benefits of technology

Through the modification of aceto-butan cellulose, the leveling and mechanical properties of the coating are significantly improved, the use of water-emulsified cellulose is reduced, the cost is reduced, and the matching of the coating and solvent-based hood paint is improved. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020513350000071
    Figure BDA0005020513350000071
  • Figure BDA0005020513350000081
    Figure BDA0005020513350000081
  • Figure BDA0005020513350000091
    Figure BDA0005020513350000091
Patent Text Reader

Abstract

The invention discloses a cellulose modified polyester polyurethane-polyacrylate aqueous dispersion for an automobile water-based finish paint and a preparation method thereof.The cellulose modified polyester polyurethane-polyacrylate aqueous dispersion is characterized in that on the basis of the characteristics of cellulose acetate butyrate, a solvent is introduced to disperse and dissolve cellulose acetate butyrate in the synthesis stage in the traditional water-based polyester polyurethane-polyacrylate synthesis process; the promotion of the cellulose on the volatilization of a dispersion medium (water and a cosolvent) and the assistance of the leveling property of the film can be fully displayed; according to the preparation method disclosed by the invention, an emulsifying function of neutralized acidic groups (organic amine) on a polyester polyurethane chain is utilized to realize a technical approach of water-based treatment of solvent type cellulose acetate butyrate, so that introduction of hydrophilic functional groups in water-emulsion cellulose acetate butyrate is reduced, and compatibility of cellulose and polyester polyurethane chain segments is fully realized; meanwhile, the application amount of the water-emulsion-shaped cellulose acetate butyrate in the formula can be reduced, the influence of introduction of the water-emulsion-shaped cellulose acetate butyrate on the coating cost is reduced, and important value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water dispersion preparation, and in particular to a cellulose modified polyester polyurethane-polyacrylate water dispersion for automobile water-based topcoat and a preparation method thereof. Background Art

[0002] At present, most of the volatile water-based automotive topcoats at home and abroad adopt the polyester polyurethane-polyacrylate system, and use the structural modification of polyurethane to adjust the physical and chemical properties of the coating film-forming material. The existing polyester polyurethane structural modification, under the premise of combining the weather resistance requirements (one of the basic requirements for the performance of automotive topcoats), basically focuses on the introduction of groups such as acrylates and silicones, and uses these groups to improve the physical and chemical parameters such as water resistance and weather resistance. However, due to the requirements of appearance and matching in the application process of coatings, the existing polyester polyurethane dispersion as a film-forming material base material has problems such as orange peel and wrinkling when biting the bottom. As for aluminum powder paint, due to the volatilization rate of the dispersion medium, the directional effect of aluminum powder is very poor, and the external water-based CAB (cellulose acetate butyrate) cannot achieve a high degree of fusion with the base resin at the molecular level, and has limited effect on the volatilization of the dispersion medium and the promotion of resin film formation. As a result, orange peel has always been a difficult problem in the coating process of volatile automotive topcoats, and matching with solvent-based topcoats is also a headache. In order to ensure a high volatilization rate of the dispersion medium of the aqueous polymer, using cellulose macromolecules to promote the flow and film formation of the dispersion is a relatively feasible technical means.

[0003] The water-based cellulose acetate butyrate currently available on the market is in the form of water emulsions, and the molecules exist in the form of micelles. The current water-based polyester polyurethane cannot reach a molecular level miscible state after being mixed with the commercially available cellulose acetate butyrate. The introduction of water-based cellulose emulsions cannot significantly improve the surface drying rate of the water-based system, and the leveling of the coating cannot be significantly improved. The introduction of a large amount of cellulose has a great impact on the performance and cost. At present, there is no ideal solution to improve the leveling of automotive water-based volatile topcoats and the matching problems with solvent-based varnishes.

[0004] For example, Chinese patent document CN201110442843.3 discloses a water-resistant and weather-resistant polyester polyurethane-polyacrylate aqueous dispersion and a preparation method thereof. The dispersion consists of three components: polyester-polyurethane, polyacrylate and water. By weight ratio: polyester-polyurethane accounts for 2.5-10%, polyacrylate accounts for 30-37.5%, and water accounts for 60%; the prepared aqueous dispersion has good hardness, toughness and water resistance, but still does not solve the leveling problem of automotive water-based volatile topcoat. Summary of the invention

[0005] In view of the deficiencies of the prior art, the object of the present invention is to provide a cellulose modified polyester polyurethane-polyacrylate aqueous dispersion for automotive water-based topcoat and a preparation method thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme:

[0007] In a first aspect, the present invention provides a method for preparing a cellulose-modified polyester polyurethane-polyacrylate aqueous dispersion for automotive water-based topcoat, comprising the following steps:

[0008] S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 200-250°C. When the acid value of the reaction system drops to 30-40 mg KOH / g, the reaction is completed, and the temperature is lowered to 50-60°C for standby use;

[0009] S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80-85°C, adding isocyanate dropwise after stirring evenly, keeping the temperature for 2-2.5h after the addition is complete, then adding monohydroxy acrylic acid monomer dropwise for end-capping, and continuing the reaction until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use;

[0010] S3, preparation of cellulose acetate butyrate solution: dissolving cellulose acetate butyrate in N-methylpyrrolidone to obtain a cellulose acetate butyrate solution for standby use;

[0011] S4. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion: add cellulose acetate butyrate solution to the above polyester polyurethane prepolymer according to the stoichiometric ratio, heat to 130-140°C, dropwise add acrylic monomer and initiator, keep warm for 3-4 hours after the dropwise addition is completed, then cool to 80-85°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, and control the theoretical residual N-methylpyrrolidone to 2-10%, continue to cool to 50-60°C, add neutralizer, the neutralization degree of carboxyl is 95-98%, add deionized water, stir and disperse evenly, and then filter to obtain cellulose modified polyester polyurethane-polyacrylate aqueous dispersion.

[0012] Preferably, in step S1, the mass ratio of diol, dibasic acid, acid anhydride and catalyst is 1-2:1-2:1-2:0.001-0.01.

[0013] Preferably, in step S1, the diol is selected from at least one of 1,4-cyclohexanedimethanol, methylpropanediol, propylene glycol, 1,6-hexanediol, and neopentyl glycol; the dibasic acid is selected from one or both of adipic acid and succinic acid; the acid anhydride is selected from one or both of phthalic anhydride and tetrahydrophthalic anhydride; and the catalyst is selected from monobutyl tin oxide.

[0014] Preferably, in step S2, when isocyanate is used to extend the polyester chain, the molar ratio of isocyanate to the hydroxyl group on the polyester chain is 1.5-2.5:1.

[0015] Preferably, in step S2, the isocyanate is selected from at least one of IPDI, HDI, and HMDI; and the monohydroxy acrylic monomer used for capping the free isocyanate is selected from one or both of hydroxypropyl acrylate and hydroxyethyl methacrylate.

[0016] Preferably, in step S3, the mass fraction of the cellulose acetate butyrate solution is 20-30%.

[0017] Preferably, in step S4, the mass ratio of the polyester polyurethane prepolymer, the cellulose acetate butyrate solution, the acrylic monomer and the initiator is 20-25:4-20:20-35:0.1-1.

[0018] Preferably, in step S4, the acrylic monomer is selected from at least one of acrylic acid, butyl acrylate, butyl methacrylate, and methyl methacrylate; the initiator is selected from one or more of benzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, and di-tert-amyl peroxide; and the neutralizer is selected from organic amines.

[0019] In a second aspect, the present invention provides a cellulose-modified polyester polyurethane-polyacrylate aqueous dispersion prepared by the above-mentioned preparation method, wherein the content of polyester polyurethane in the prepared cellulose-modified polyester polyurethane-polyacrylate aqueous dispersion is 20-25wt%, the content of cellulose acetate is 1-5wt%, and the content of polyacrylate is 20-35wt%.

[0020] In a third aspect, the present invention also provides the use of the above-mentioned cellulose modified polyester polyurethane-polyacrylate aqueous dispersion in automotive water-based topcoat.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) Based on the characteristics of cellulose acetate, the present invention introduces solvent-dispersed cellulose acetate in the synthesis stage during the traditional water-based polyester-polyurethane-polyacrylate synthesis process. At this time, cellulose acetate and polyester chains, polyurethane chains and subsequent modifiers can form molecular interpenetration, and each polymer chain segment can fully display its molecular properties. The promotion of cellulose to the volatilization of the dispersion medium (water, co-solvent) and the assistance to the film leveling can be fully displayed; the present invention utilizes the emulsification function (organic amine) of the acidic groups on the polyester chain and the polyurethane chain after neutralization to achieve the technical approach of making the solvent-based cellulose acetate water-based, which not only reduces the introduction of hydrophilic functional groups in the water-emulsified cellulose acetate, but also fully realizes the compatibility of cellulose with polyurethane and polyester segments. At the same time, it can reduce the amount of water-emulsified cellulose acetate used in the formula, and reduce the impact of the introduction of water-emulsified cellulose acetate on the coating cost, which is of great value.

[0023] (2) Polyester polyurethane is the main film material for solving the mechanical properties of automobile topcoat coatings. Compared with acrylic polymers, polyester polyurethane not only provides decorative properties for the coating appearance, but also has conventional mechanical properties that acrylic polymers do not have. It also has unique advantages in forward and reverse impact and cupping tests, and coating compatibility. In addition to utilizing polyurethane to extend the chain grafting of polyester to improve the compatibility of different structural resin segments, the present invention also increases the amount of polyester polyurethane segments to increase the decorative appearance of the coating and strengthen the mechanical properties of the coating. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.

[0025] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.

[0026] A method for preparing a cellulose-modified polyester polyurethane-polyacrylate aqueous dispersion for automotive water-based topcoat comprises the following steps:

[0027] S1. Preparation of polyester intermediates

[0028] Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 200-250°C. When the acid value of the reaction system drops to 30-40 mg KOH / g, the reaction is completed, and the temperature is lowered to 50-60°C for standby use.

[0029] In this step, the mass ratio of diol, dibasic acid, acid anhydride and catalyst is 1-2:1-2:1-2:0.001-0.01.

[0030] Wherein, the diol is selected from at least one of 1,4-cyclohexanedimethanol, methyl propanediol, propylene glycol, 1,6-hexanediol and neopentyl glycol.

[0031] The dibasic acid is selected from one or both of adipic acid and succinic acid.

[0032] The acid anhydride is selected from one or both of phthalic anhydride and tetrahydrophthalic anhydride.

[0033] The catalyst is selected from monobutyltin oxide.

[0034] S2. Preparation of polyester polyurethane prepolymer

[0035] In the reactor, the synthesized polyester intermediate is used as the base, the temperature is kept at 80-85°C, isocyanate is added dropwise after stirring evenly, and the temperature is kept for 2-2.5 hours after the addition is completed. Then, the monohydroxy acrylic monomer is added dropwise for end-capping, and the reaction is continued until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use.

[0036] In this step, the amount of isocyanate added is based on a molar ratio of -NCO in the isocyanate / -OH group in the polyester of 1.5-2.5:1, more preferably 1.5-2:1.

[0037] Wherein, the isocyanate is selected from at least one of IPDI, HDI and HMDI.

[0038] The monohydroxy acrylic monomer is selected from one or both of hydroxypropyl acrylate and hydroxyethyl methacrylate.

[0039] S3. Preparation of cellulose acetate butyrate solution

[0040] Dissolve cellulose acetate butyrate in N-methylpyrrolidone to obtain a cellulose acetate butyrate solution for later use.

[0041] In this step, the mass fraction of the cellulose acetate butyrate solution is 20-30%, for example, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% can be selected, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] S4. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion

[0043] The cellulose acetate butyrate solution is added to the polyester polyurethane prepolymer according to the stoichiometric ratio, the temperature is raised to 130-140° C., acrylic monomer and initiator are added dropwise, and the temperature is kept for 3-4 hours after the addition is completed, and then the temperature is lowered to 80-85° C., and N-methylpyrrolidone and free acrylic monomer are extracted by vacuum distillation, and the theoretical residual N-methylpyrrolidone is controlled at 2-10%. The temperature is further lowered to 50-60° C., a neutralizer is added, and the neutralization degree of the carboxyl group is 95-98%, and deionized water is added. After stirring and dispersing evenly, it is filtered to obtain a cellulose-modified polyester polyurethane-polyacrylate aqueous dispersion.

[0044] In this step, the mass ratio of polyester polyurethane prepolymer, cellulose acetate butyrate solution, acrylic monomer and initiator is 20-25:4-20:20-35:0.1-1, and more preferably 22-24:10-15:25-30:0.3-0.6.

[0045] Specifically, the acrylic monomer is selected from at least one of acrylic acid, butyl acrylate, butyl methacrylate, and methyl methacrylate.

[0046] Specifically, the initiator is selected from one or more of benzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, and di-tert-amyl peroxide.

[0047] Specifically, the neutralizing agent is selected from organic amines, for example, N,N-dimethylethanolamine or triethylamine.

[0048] The present invention is further described below by means of specific examples, wherein the model of cellulose acetate butyrate used in the present invention is CAB551, and the compositions of the materials in Examples 1-5 of the present invention and Comparative Example 1 are shown in Table 1 below. Compared with Example 1, Comparative Example 1 does not contain 25 wt % cellulose acetate butyrate solution;

[0049] Table 1 Composition of materials in Examples 1-5 and Comparative Example 1 (unit: g)

[0050]

[0051]

[0052]

[0053] Example 1

[0054] Add each material according to the formula in Example 1 in Table 1, and the specific preparation process is as follows:

[0055] S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 240°C. When the acid value of the reaction system drops to 35 mg KOH / g, the reaction is completed, and the temperature is lowered to 60°C for standby use;

[0056] S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80°C, adding isocyanate dropwise after stirring evenly, and the addition is completed within 30 minutes, and the temperature is kept for 2 hours, and then monohydroxy acrylic acid monomer is added dropwise for end-capping, and the reaction is continued until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use;

[0057] S3, preparation of cellulose acetate butyrate solution: dissolving cellulose acetate butyrate in N-methylpyrrolidone to prepare a 25 wt % cellulose acetate butyrate solution for standby use;

[0058] S4. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion: add cellulose acetate butyrate solution to the above polyester polyurethane prepolymer according to the stoichiometric ratio, heat to 130°C, dropwise add acrylic monomer and initiator, add the mixture over 2 hours, keep warm for 3 hours, then cool to 80°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, the theoretical residual N-methylpyrrolidone is controlled at 5%, continue to cool to 50°C, add neutralizer, the neutralization degree of carboxyl is 98%, add deionized water, stir and disperse evenly, and filter to obtain cellulose modified polyester polyurethane-polyacrylate aqueous dispersion.

[0059] Example 2

[0060] Add each material according to the formula in Example 2 in Table 1, and the specific preparation process is as follows:

[0061] S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 200°C. When the acid value of the reaction system drops to 38mg KOH / g, the reaction is completed, and the temperature is lowered to 60°C for standby use;

[0062] S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80°C, adding isocyanate dropwise after stirring evenly, and the addition is completed within 30 minutes, and the temperature is kept for 2 hours, and then monohydroxy acrylic acid monomer is added dropwise for end-capping, and the reaction is continued until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use;

[0063] S3, preparation of cellulose acetate butyrate solution: dissolving cellulose acetate butyrate in N-methylpyrrolidone to prepare a 25 wt % cellulose acetate butyrate solution for standby use;

[0064] S4. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion: add cellulose acetate butyrate solution to the above polyester polyurethane prepolymer according to the stoichiometric ratio, heat to 130°C, dropwise add acrylic monomer and initiator, add the mixture over 2 hours, keep warm for 3 hours, then cool to 80°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, the theoretical residual N-methylpyrrolidone is controlled at 5%, continue to cool to 50°C, add neutralizer, the neutralization degree of carboxyl is 98%, add deionized water, stir and disperse evenly, and filter to obtain cellulose modified polyester polyurethane-polyacrylate aqueous dispersion.

[0065] Example 3

[0066] Add each material according to the formula in Example 3 in Table 1, and the specific preparation process is as follows:

[0067] S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 250°C. When the acid value of the reaction system drops to 40mg KOH / g, the reaction is completed, and the temperature is lowered to 60°C for standby use;

[0068] S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80°C, adding isocyanate dropwise after stirring evenly, and the addition is completed within 30 minutes, and the temperature is kept for 2 hours, and then monohydroxy acrylic acid monomer is added dropwise for end-capping, and the reaction is continued until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use;

[0069] S3, preparation of cellulose acetate butyrate solution: dissolving cellulose acetate butyrate in N-methylpyrrolidone to prepare a 25 wt % cellulose acetate butyrate solution for standby use;

[0070] S4. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion: add cellulose acetate butyrate solution to the above polyester polyurethane prepolymer according to the stoichiometric ratio, heat to 130°C, dropwise add acrylic monomer and initiator, add the mixture over 2 hours, keep warm for 3 hours, then cool to 80°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, the theoretical residual N-methylpyrrolidone is controlled at 5%, continue to cool to 50°C, add neutralizer, the neutralization degree of carboxyl is 98%, add deionized water, stir and disperse evenly, and filter to obtain cellulose modified polyester polyurethane-polyacrylate aqueous dispersion.

[0071] Example 4

[0072] Add the materials according to the formula in Example 4 in Table 1, and the specific preparation process is as follows:

[0073] S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 240°C. When the acid value of the reaction system drops to 35 mg KOH / g, the reaction is completed, and the temperature is lowered to 60°C for standby use;

[0074] S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80°C, adding isocyanate dropwise after stirring evenly, and the addition is completed within 30 minutes, and the temperature is kept for 2 hours, and then monohydroxy acrylic acid monomer is added dropwise for end-capping, and the reaction is continued until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use;

[0075] S3, preparation of cellulose acetate butyrate solution: dissolving cellulose acetate butyrate in N-methylpyrrolidone to prepare a 25 wt % cellulose acetate butyrate solution for standby use;

[0076] S4. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion: add cellulose acetate butyrate solution to the above polyester polyurethane prepolymer according to the stoichiometric ratio, heat to 130°C, dropwise add acrylic monomer and initiator, add the mixture over 2 hours, keep warm for 3 hours, then cool to 80°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, the theoretical residual N-methylpyrrolidone is controlled at 5%, continue to cool to 50°C, add neutralizer, the neutralization degree of carboxyl is 98%, add deionized water, stir and disperse evenly, and filter to obtain cellulose modified polyester polyurethane-polyacrylate aqueous dispersion.

[0077] Example 5

[0078] Add each material according to the formula in Example 5 in Table 1, and the specific preparation process is as follows:

[0079] S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 240°C. When the acid value of the reaction system drops to 36 mg KOH / g, the reaction is completed, and the temperature is lowered to 60°C for standby use;

[0080] S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80°C, adding isocyanate dropwise after stirring evenly, and the addition is completed within 30 minutes, and the temperature is kept for 2 hours, and then monohydroxy acrylic acid monomer is added dropwise for end-capping, and the reaction is continued until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use;

[0081] S3. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion: add cellulose acetate butyrate solution to the above polyester polyurethane prepolymer according to the stoichiometric ratio, heat to 130°C, dropwise add acrylic monomer and initiator, add the mixture over 2 hours, keep warm for 3 hours, then cool to 80°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, the theoretical residual N-methylpyrrolidone is controlled at 5%, continue to cool to 50°C, add neutralizer, the neutralization degree of carboxyl is 98%, add deionized water, stir and disperse evenly, and filter to obtain cellulose modified polyester polyurethane-polyacrylate aqueous dispersion.

[0082] Comparative Example 1

[0083] Add each material according to the formula in Comparative Example 1 in Table 1, and the specific preparation process is as follows:

[0084] S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 240°C. When the acid value of the reaction system drops to 40mg KOH / g, the reaction is completed, and the temperature is lowered to 60°C for standby use;

[0085] S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80°C, adding isocyanate dropwise after stirring evenly, and the addition is completed within 30 minutes, and the temperature is kept for 2 hours, and then monohydroxy acrylic acid monomer is added dropwise for end-capping, and the reaction is continued until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use;

[0086] S3. Preparation of polyester polyurethane-polyacrylate aqueous dispersion: Heat the polyester polyurethane prepolymer to 130°C, add acrylic monomer and initiator dropwise, complete the addition within 2 hours, keep warm for 3 hours, then cool to 80°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, and control the theoretical residual N-methylpyrrolidone to 5%, continue to cool to 50°C, add neutralizer, the neutralization degree of carboxyl is 98%, add deionized water, stir and disperse evenly, and filter to obtain polyester polyurethane-polyacrylate aqueous dispersion.

[0087] The cellulose modified polyester polyurethane-polyacrylate aqueous dispersion prepared in Examples 1-5 and Comparative Example 1 was used to prepare the coating. The coating formulation and performance test results are shown in Table 2:

[0088] Table 2

[0089]

[0090] Among them, the model of the substrate wetting agent is Digao 4100; the model of the water-based defoaming agent is byk024; and the model of the water-based dispersant is byk104S.

[0091] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.

Claims

1. A method for preparing a cellulose-modified polyester polyurethane-polyacrylate aqueous dispersion for automotive water-based topcoat, characterized in that: The steps include: S1. Preparation of polyester intermediate: Add diol, dibasic acid and acid anhydride to N-methylpyrrolidone, then add catalyst, stir and react at 200-250°C. When the acid value of the reaction system drops to 30-40 mg KOH / g, the reaction is completed, and the temperature is lowered to 50-60°C for standby use; S2. Preparation of polyester polyurethane prepolymer: using the synthesized polyester intermediate as the base in the reactor, keeping the temperature at 80-85°C, adding isocyanate dropwise after stirring evenly, keeping the temperature for 2-2.5h after the addition is complete, then adding monohydroxy acrylic acid monomer dropwise for end-capping, and continuing the reaction until the free NCO group disappears to obtain a polyester polyurethane prepolymer for standby use; S3, preparation of cellulose acetate butyrate solution: dissolving cellulose acetate butyrate in N-methylpyrrolidone to obtain a cellulose acetate butyrate solution for standby use; S4. Preparation of cellulose modified polyester polyurethane-polyacrylate aqueous dispersion: add cellulose acetate butyrate solution to the above polyester polyurethane prepolymer according to the stoichiometric ratio, heat to 130-140°C, dropwise add acrylic monomer and initiator, keep warm for 3-4 hours after the dropwise addition is completed, then cool to 80-85°C, extract N-methylpyrrolidone and free acrylic monomer by vacuum distillation, and control the theoretical residual N-methylpyrrolidone to 2-10%, continue to cool to 50-60°C, add neutralizer, the neutralization degree of carboxyl is 95-98%, add deionized water, stir and disperse evenly, and then filter to obtain cellulose modified polyester polyurethane-polyacrylate aqueous dispersion.

2. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of diol, dibasic acid, acid anhydride and catalyst is 1-2:1-2:1-2:0.001-0.

01.

3. The preparation method according to claim 1, characterized in that: In step S1, the diol is selected from at least one of 1,4-cyclohexanedimethanol, methyl propanediol, propylene glycol, 1,6-hexanediol, and neopentyl glycol; the dibasic acid is selected from one or both of adipic acid and succinic acid; the acid anhydride is selected from one or both of phthalic anhydride and tetrahydrophthalic anhydride; and the catalyst is selected from monobutyl tin oxide.

4. The preparation method according to claim 1, characterized in that: In step S2, when isocyanate is used to extend the polyester chain, the molar ratio of the isocyanate to the hydroxyl groups on the polyester chain is 1.5-2.5:

1.

5. The preparation method according to claim 1, characterized in that: In step S2, the isocyanate is selected from at least one of IPDI, HDI, and HMDI; and the monohydroxy acrylic monomer used for capping the free isocyanate after isocyanate chain extension is selected from one or both of hydroxypropyl acrylate and hydroxyethyl methacrylate.

6. The preparation method according to claim 1, characterized in that: In step S3, the mass fraction of the cellulose acetate butyrate solution is 20-30%.

7. The preparation method according to claim 1, characterized in that: In step S4, the mass ratio of polyester polyurethane prepolymer, cellulose acetate butyrate solution, acrylic monomer and initiator is 20-25:4-20:20-35:0.1-1.

8. The preparation method according to claim 1, characterized in that: In step S4, the acrylic monomer is selected from at least one of acrylic acid, butyl acrylate, butyl methacrylate, and methyl methacrylate; the initiator is selected from one or more of benzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, and di-tert-amyl peroxide; and the neutralizer is selected from organic amines.

9. The cellulose modified polyester polyurethane-polyacrylate aqueous dispersion prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The prepared cellulose modified polyester polyurethane-polyacrylate aqueous dispersion has a polyester polyurethane content of 20-25wt%, a cellulose acetate butyrate content of 1-5wt%, and a polyacrylate content of 20-35wt%.

10. Use of the cellulose modified polyester polyurethane-polyacrylate aqueous dispersion as claimed in claim 9 in automotive water-based topcoat.

Citation Information

Patent Citations

  • Method for synthesizing cellulose nitrate-polyurethane-polyacrylic acid(polyacrylate) composite emulsion

    CN101235125A

  • Water-resistant and weather-resistant polyester polyurethane-polyacrylate aqueous dispersion and preparation method thereof

    CN102516466A

  • Weather-resisting type single-coating powder paint with metal pattern effect

    CN106280914A

  • Core-shell type polyester-acrylic emulsion as well as preparation method and application thereof

    CN111690097A

  • Cellulose modified polyester acrylate aqueous dispersion as well as preparation method and application thereof

    CN117683186A