Cr3 + activated beta-Ga2O3 with interstitial oxygen ions and near-infrared luminescent material with derivative structure of beta-Ga2O3 as well as preparation method and application of near-infrared luminescent material
By introducing gap oxygen ions into β-Ga2O3 and its derivative structure, the problem of insufficient efficiency and thermal stability of near-infrared luminescent materials is solved, and efficient and adjustable near-infrared luminescent materials are achieved, which is suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202410952622.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing near-infrared luminescent materials have low efficiency, insufficient thermal stability, and difficult to achieve spectral adjustment, which limits their application in health testing, food testing and other fields.
By introducing gap oxygen ions into β-Ga2O3 and its derivative structure, the non-equivalent substitution of the trivalent ions Ga3+, Sc3+, and In3+ by tetravalent ions Ge4+, Sn4+ or Ti4+, the structural rigidity is improved and the non-unit between Cr3+ ions is suppressed. Radiation transition to improve luminous intensity and thermal stability.
The luminescence intensity is increased to 1.8 times that of the original material, the thermal stability is increased by 40%, and the emission peak position and spectral peak shape can be adjusted. It is suitable for near-infrared emissions of different wavelengths, and the external quantum efficiency reaches 40%-53%.
Smart Images

Figure CN118909626A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of luminescent materials and particularly relates to a Cr 3+ Activated beta-Ga2O3 with interstitial oxygen ions and near-infrared luminescent materials of its derived structure, as well as preparation methods and applications thereof. Background Art
[0002] In recent years, with the rapid development of near-infrared spectroscopy technology in the fields of facial recognition, iris recognition, security monitoring, laser radar, health detection, 3D sensing, etc., near-infrared LEDs have also become the focus of international research due to their advantages such as good directivity, large penetration depth, less interference, low power consumption and small size. At present, the technology to achieve LED near-infrared emission is mainly obtained through near-infrared chips, but this technology is costly, immature, and the emission wavelength has a narrow half-peak width, so its application is limited to tube emission, security and other fields. Another technology to achieve LED infrared emission is to use a blue light chip to excite near-infrared phosphors. This near-infrared emission technology has the advantages of low cost and wide-spectrum emission, and is widely used in plant lighting, standard light sources, health detection and other fields. At present, the development of this near-infrared LED is still in a relatively preliminary stage. For the currently known near-infrared luminescent materials, there are still problems such as low efficiency and insufficient thermal stability. In addition, in health detection, food detection and other aspects, since different detection substances and environments have different optimal absorption positions for near-infrared light, near-infrared luminescent materials with adjustable spectra are also worth studying. Therefore, the development of high-performance, high-efficiency, and adjustable broadband near-infrared luminescent phosphors is of great significance.
[0003] At present, the Cr 3+ There are many reports on the quantum efficiency and thermal stability of doped near-infrared luminescent materials, but the process of improving performance through equivalent substitution is usually accompanied by changes in the excitation and emission spectra, and none of them solves the problem of the difficulty in improving the luminescence performance of existing near-infrared fluorescent materials. 3+ In doped near-infrared luminescent materials, interstitial ions are formed by non-equivalent substitution, such as O 2- There have been no similar reports on methods for improving the luminous efficiency and thermal stability by reducing the gap, etc. Summary of the invention
[0004] In view of this, the present invention is based on Cr 3+ Activated β-Ga2O3 and its derivative structure near-infrared luminescent materials provide a Cr 3+ Activated β-Ga2O3 with interstitial oxygen ions and its derived structure near-infrared luminescent material and its preparation method and application. 4+ Sn 4+ or Ti4+ For trivalent ions Ga 3+ Sc 3+ 、In 3+ The non-equivalent substitution of Cr generates interstitial oxygen ions in the structure, which improves the structural rigidity and inhibits Cr 3+ The non-radiative transition between ions significantly improves the luminescence intensity and thermal stability of materials without interstitial oxygen ions. The near-infrared luminescent material provided by the present invention can obtain near-infrared light emission under the excitation of near-ultraviolet or blue light, and a series of near-infrared luminescent materials with different emission peak positions, spectral peak shapes and half-peak widths can be obtained by controlling the components.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] In one aspect, the present invention provides a Cr 3+ Activated with gap O 2- β-Ga2O3 and its derivative structure near-infrared luminescent material, the chemical structure of the luminescent material is A x B y Cr z O 3+a , wherein: A is one or more of the trivalent cations Ga, Sc, and In, and A must contain Ga, B is one of the tetravalent cations Ge, Sn, and Ti, 0 <y≤0.2,0<z≤0.1,x+y+z=2,0<a≤0.1。
[0007] In the above technical solution, further, the molar percentage of Ga in the luminescent material is >50%.
[0008] In the above technical solution, further, the near-infrared luminescent material belongs to the monoclinic crystal system, and the space point group is C2 / m.
[0009] Another aspect of the present invention provides a method for preparing the above-mentioned near-infrared luminescent material, the method comprising the following steps:
[0010] Step 1: According to the chemical formula A x B y Cr z O 3+a Weigh the A source, B source, and Cr source according to the stoichiometric ratio of each chemical composition; Step 2: Grind the raw materials and mix them to obtain a mixture;
[0011] Step 3: sintering the mixture obtained in step 2 in a muffle furnace in stages, and then cooling to room temperature to obtain a sintered product;
[0012] Step 4: Grind the sintered product obtained in step 3 into powder to obtain a near-infrared luminescent material.
[0013] In the above technical solution, further, the A source is one or more of the oxides, carbonates, and nitrates of metal A; the B source is one or more of the oxides, carbonates, and nitrates of metal B; and the Cr source is one or more of chromium oxide, chromium carbonate, and chromium nitrate.
[0014] In the above technical solution, further, in step 3, the staged sintering is: firstly increase the temperature to 600-800°C at a heating rate of 5°C / min, keep warm for 0.5-1h, then increase the temperature to 1200-1500°C at a heating rate of 5°C / min, keep warm for 4-8 hours.
[0015] The present invention also provides a near-infrared LED device, comprising an LED chip, wherein the LED chip is coated with the near-infrared luminescent material according to any one of claims 1 to 3.
[0016] In the above technical solution, further, the light emission wavelength of the LED chip is 300nm-600nm.
[0017] The beneficial effects of the present invention are:
[0018] 1) The present invention conducts the tetravalent ion Ge in β-Ga2O3 and its derivative structure near-infrared luminescent materials 4+ Sn 4+ or Ti 4+ For trivalent ions Ga 3+ Sc 3+ 、In 3+ The non-equivalent substitution of ions introduces interstitial oxygen ions and maintains the charge balance of the system, thereby improving the luminescence intensity and thermal stability without changing the excitation and emission spectra of the luminescent material.
[0019] 2) In Cr 3+ In the activated β-Ga2O3 and its derivative structure (Ga, Sc, In)2O3, compared with the luminescent materials without interstitial oxygen structure, the luminescence intensity and thermal stability can be improved by introducing interstitial oxygen structure. In different materials, by introducing suitable tetravalent cations and constructing interstitial oxygen structure, the luminescence intensity can be as high as 1.8 times that of the original luminescent material, and the luminescence thermal stability (the ratio of the luminescence intensity at 150°C to the luminescence intensity at room temperature) can be improved by about 40%.
[0020] 3) The near-infrared luminescent material with interstitial oxygen structure of the present invention has a wide excitation band (250nm-600nm), can be effectively excited by ultraviolet light and near-ultraviolet light, and has an emission spectrum of near-infrared emission in the range of 600nm-950nm, and its emission peak can be adjusted in the range of 680nm-850nm, and the half-height width can be adjusted in the range of 25nm-170nm.
[0021] 4) The near-infrared phosphor with interstitial oxygen structure of the present invention has excellent luminous intensity. For embodiments emitting at different wavelengths, an external quantum efficiency of 40%-53% can be achieved through the design of the interstitial oxygen structure.
[0022] 5) The green phosphor of the present invention is prepared by a high-temperature solid-phase method. The uniformly mixed reactants are in close contact with each other. At high temperatures, the ions near the contact surface have enough energy to break free from the constraints of their inherent lattices and diffuse. Through the mutual diffusion of different atoms and the formation and growth of crystal nuclei, a luminescent material is formed. The preparation process is simple, low-cost, non-toxic, pollution-free, and can be industrially produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 XRD spectra of the near-infrared luminescent materials prepared in Example 5 and Comparative Example 2;
[0024] Figure 2 This is a comparison chart of emission spectra of near-infrared luminescent materials prepared in Example 5 and Comparative Example 2 under 450nm excitation;
[0025] Figure 3 This is a comparison chart of the luminescence intensity versus temperature curves of the near-infrared luminescent materials prepared in Example 5 and Comparative Example 2 under 450nm excitation;
[0026] Figure 4 These are the quantum efficiency test results of the near-infrared luminescent materials prepared in Example 5 and Comparative Example 2. DETAILED DESCRIPTION
[0027] The present invention is further described below with reference to specific embodiments and drawings, which are intended to explain the present invention rather than to limit it.
[0028] Unless otherwise specified, the materials used in the embodiments of the present invention can be obtained through commercial channels or prepared according to conventional methods well known to those skilled in the art.
[0029] Example 1
[0030] After weighing Ga2O3, GeO2, and Cr2O3 according to a formula in which the molar ratio of Ga element, Ge element, and Cr element is 1.965:0.03:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1400°C at a heating rate of 5°C / min, and kept warm for 6 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0031] Example 2
[0032] After weighing Ga2O3, GeO2, and Cr2O3 according to a formula in which the molar ratio of Ga element, Ge element, and Cr element is 1.935:0.06:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1400°C at a heating rate of 5°C / min, and kept warm for 6 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0033] Example 3
[0034] After weighing Ga2O3, TiO2, and Cr2O3 according to a formula in which the molar ratio of Ga element, Ti element, and Cr element is 1.935:0.06:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1400°C at a heating rate of 5°C / min, and kept warm for 6 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0035] Example 4
[0036] Ga2O3, Sc2O3, GeO2, and Cr2O3 are weighed according to a formula in which the molar ratio of Ga element, Sc element, Ge element, and Cr element is 1.565:0.4:0.03:0.005, and the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1h; then the temperature is increased to 1500°C at a heating rate of 5°C / min, and kept warm for 8 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0037] Example 5
[0038] After weighing Ga2O3, Sc2O3, GeO2, and Cr2O3 according to a formula in which the molar ratio of Ga element, Sc element, Ge element, and Cr element is 1.535:0.4:0.06:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1500°C at a heating rate of 5°C / min, and kept warm for 8 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0039] Example 6
[0040] After weighing Ga2O3, Sc2O3, GeO2, and Cr2O3 according to a formula in which the molar ratio of Ga element, Sc element, Ge element, and Cr element is 1.395:0.4:0.2:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1h; then the temperature is increased to 1500°C at a heating rate of 5°C / min, and kept warm for 8 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0041] Example 7
[0042] After weighing Ga2O3, In2O3, SnO2, and Cr2O3 according to a formula in which the molar ratio of Ga element, In element, Sn element, and Cr element is 1.565:0.4:0.03:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1500°C at a heating rate of 5°C / min, and kept warm for 8 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0043] Example 8
[0044] Ga2O3, In2O3, SnO2, and Cr2O3 are weighed according to a formula in which the molar ratio of Ga element, In element, Ti element, and Cr element is 1.535:0.4:0.06:0.005, and the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1h; then the temperature is increased to 1500°C at a heating rate of 5°C / min, and kept warm for 8 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0045] Example 9
[0046] After weighing Ga2O3, Sc2(CO3)3, GeO2, and Cr2(CO3)3 according to a formula in which the molar ratio of Ga, Sc, Ge, and Cr is 1.3:0.4:0.2:0.1, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1h; then the temperature is increased to 1200°C at a heating rate of 5°C / min, kept warm for 4 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0047] Example 10
[0048] Ga2O3, Sc2(CO3)3, TiO2 and Cr2(CO3)3 were weighed according to a formula in which the molar ratio of Ga, Sc, Ge and Cr was 1.44:0.4:0.06:0.1, and the above raw materials were fully ground and mixed to obtain a mixture; the above mixture was placed in a corundum crucible and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature was first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1h; then the temperature was increased to 1200°C at a heating rate of 5°C / min, and kept warm for 4 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product was crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0049] Comparative Example 1
[0050] After weighing Ga2O3 and Cr2O3 according to a formula in which the molar ratio of Ga element to Cr element is 1.995:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of introducing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1400°C at a heating rate of 5°C / min, kept warm for 6 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, passed through a 300-mesh sieve, and a near-infrared phosphor is obtained.
[0051] Comparative Example 2
[0052] After weighing Ga2O3, Sc2O3, and Cr2O3 according to a formula in which the molar ratio of Ga element, Sc element, and Cr element is 1.595:0.4:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1500°C at a heating rate of 5°C / min, and kept warm for 8 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0053] Comparative Example 3
[0054] After weighing Ga2O3, In2O3, and Cr2O3 according to a formula in which the molar ratio of Ga element, In element and Cr element is 1.595:0.4:0.005, the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible, and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1500°C at a heating rate of 5°C / min, and kept warm for 8 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0055] Comparative Example 4
[0056] Ga2O3, Sc2(CO3)3 and Cr2(CO3)3 are weighed according to a formula in which the molar ratio of Ga element, Sc element and Cr element is 1.5:0.4:0.1, and the above raw materials are fully ground and mixed to obtain a mixture; the above mixture is placed in a corundum crucible and then put into a tubular furnace, and under the condition of passing a reducing atmosphere composed of 5% H2 and 95% N2 by volume, the temperature is first increased to 800°C at a heating rate of 5°C / min, and kept warm for 1 hour; then the temperature is increased to 1200°C at a heating rate of 5°C / min, and kept warm for 4 hours, and naturally cooled to room temperature to obtain a sintered product; the sintered product is crushed into powder, and passed through a 300-mesh sieve to obtain a near-infrared phosphor.
[0057] The near-infrared luminescent materials prepared in Examples 1-10 and Comparative Examples 1-4 were respectively tested for photoluminescence performance, and their relative luminescence intensity and thermal stability under 450nm wavelength excitation were measured. The results are shown in Table 1 below.
[0058] Table 1 Emission intensity and thermal stability test results of Examples 1-10 and Comparative Examples 1-4
[0059]
[0060]
[0061] Figure 1 The XRD patterns of the near-infrared luminescent materials obtained in Example 5 and Comparative Example 2 are as follows: Figure 1 It can be seen that after comparison with the standard card of Ga2O3, when a small amount of tetravalent ions are doped, its crystal structure will not be changed, and no other impurity phases will be produced.
[0062] Figure 2 The comparison diagram of the emission spectra of the near-infrared luminescent materials obtained in Example 5 and Comparative Example 2 is shown in FIG. Figure 2It can be seen that the intensity is significantly improved by doping with Ge, and the shape of its emission spectrum does not change significantly.
[0063] Figure 3 The luminescence intensity of the near-infrared luminescent materials prepared in Example 5 and Comparative Example 2 varies with temperature. When the temperature rises from room temperature (25°C) to 225°C, it can be seen that the thermal stability is significantly improved by doping with Ge.
[0064] Figure 4 The quantum efficiency test results of the near-infrared luminescent materials prepared in Example 5 and Comparative Example 2 are as follows: Figure 4 It can be seen that the quantum efficiency is significantly improved by doping with Ge.
[0065] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined in the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.
Claims
1. A Cr 3+ Activated with gap O 2- β-Ga 2 O 3 Near-infrared luminescent materials and their derivative structures, It is characterized in that The chemical structural formula of the luminescent material is A x B y Cr z O 3+a , wherein: A is one or more of the trivalent cations Ga, Sc, and In, and A must contain Ga, B is one of the tetravalent cations Ge, Sn, and Ti, 0 <y≤0.2,0<z≤0.1,x+y+z=2,0<a≤0.1。 2. The near-infrared luminescent material according to claim 1, It is characterized in that The molar percentage of Ga in the light-emitting material is greater than 50%.
3. The near-infrared luminescent material according to claim 1, It is characterized in that The near-infrared luminescent material belongs to the monoclinic crystal system, and the space point group is C2 / m.
4. A method for preparing the near-infrared luminescent material according to any one of claims 1 to 3, It is characterized in that The method comprises the following steps: Step 1: According to the chemical formula A x B y Cr z O 3+a Weigh the A source, B source, and Cr source according to the stoichiometric ratio of each chemical composition; Step 2: Grind the raw materials and mix them to obtain a mixture; Step 3: sintering the mixture obtained in step 2 in a muffle furnace in stages, and then cooling to room temperature to obtain a sintered product; Step 4: Grind the sintered product obtained in step 3 into powder to obtain a near-infrared luminescent material.
5. The preparation method according to claim 4, It is characterized in that The A source is one or more of the oxide, carbonate, and nitrate of metal A; The B source is one or more of an oxide, a carbonate, and a nitrate of metal B; The Cr source is one or more of chromium oxide, chromium carbonate and chromium nitrate.
6. The preparation method according to claim 4, It is characterized in that In step 3, the staged sintering is as follows: firstly, the temperature is raised to 600-800°C at a heating rate of 5°C / min, and kept at that temperature for 0.5-1h, and then the temperature is raised to 1200-1500°C at a heating rate of 5°C / min, and kept at that temperature for 4-8 hours.
7. A near-infrared LED device, It is characterized in that It comprises an LED chip, on which the near-infrared luminescent material according to any one of claims 1 to 3 is coated.
8. The near-infrared LED device according to claim 7, It is characterized in that The light emission wavelength of the LED chip is 300nm-600nm.
Citation Information
Patent Citations
Beta-gallium oxide structure near-infrared wide-spectrum fluorescent powder and preparation method thereof
CN113956873A
Near-infrared emission enhanced Ga2O3: Cr < 3 + > luminescent material and preparation method thereof
CN115595152A
Preparation and application of gallium germanate near-infrared luminescent material
CN118256238A