Nickel-based superalloy composite material reinforced by nano ceramic particles and preparation method of nickel-based superalloy composite material
By uniformly dispersing nanoceramic particles in nickel-based high-temperature alloys, the problems of large phase size and surface pollution of traditional high-temperature alloys are solved, which significantly improves high-temperature wear resistance and tensile strength, achieves fine crystal strengthening effect, and reduces preparation cost .
Patent Information
- Application Number
- CN202410964542.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
After the introduction of the reinforced phase, traditional high-temperature alloys have problems with large reinforced phase size, differences in thermal properties and matrix, surface pollution and agglomeration, resulting in a decrease in the mechanical properties of the materials and it is difficult to further improve the comprehensive mechanical properties.
Nanoceramic particles (TiC and TiB2) are uniformly dispersed in nickel-based high-temperature alloys through prefabricated aluminum-based intermediate alloys, and nanoceramic particles are prepared by ball milling and ultrasonic oscillation treatment, combining vacuum induction smelting, electroslag remelting, homogenization treatment and Through forging and other processes, nickel-based high-temperature alloy composite materials with enhanced nanoceramic particles were prepared.
While maintaining the plasticity of the material, the high-temperature wear resistance, yield strength and tensile strength are significantly improved, the surface pollution of nanoparticles is avoided, uniform dispersion of nanoparticles and fine crystal strengthening are achieved, and the material preparation cost is reduced.
Smart Images

Figure CN118910471A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a nano-ceramic particle reinforced nickel-based high-temperature alloy composite material and also relates to a preparation method of the high-temperature alloy composite material. Background Art
[0002] High-temperature alloys, also known as heat-resistant alloys, can withstand complex stresses under oxidation and gas corrosion conditions at 600 to 1100°C and can work reliably for a long time. They are mainly used for the hot end components of aircraft engines and are also important materials in the fields of aerospace, energy, transportation, chemical industry, hot working molds, etc. The strengthening methods of traditional high-temperature alloys are mainly solid solution strengthening, precipitation strengthening, and grain boundary strengthening. Solid solution strengthening and precipitation strengthening mainly depend on the types of alloying elements and their content ratios. However, after decades of research and development, the elements and composition systems of high-temperature alloys have tended to be optimal, and it is difficult to further strengthen high-temperature alloys through these two methods. Grain boundary strengthening is mainly achieved by grain refinement. Commercial large-size high-temperature alloys use plastic processing and heat treatment as grain refinement methods. The average grain size can generally be refined to the micron level and it is currently difficult to continue to break through, so the potential for grain boundary strengthening is limited.
[0003] In order to further improve the comprehensive mechanical properties of traditional high-temperature alloys, a reinforcing phase with stable chemical properties is added to the alloy matrix. When it is evenly distributed in the matrix, it can hinder the dislocation movement of atoms and play a role in dispersion strengthening. However, the current process of strengthening high-temperature alloys by introducing a second phase often has the following problems: First, the reinforcing phase is large in size (above the micron level), and its thermal and mechanical properties are significantly different from the matrix alloy structure, which makes the interface between the two phases easy to become a crack source. Secondly, the surface of the reinforcing phase is easily contaminated during preparation, storage, transportation and alloy smelting, thereby reducing the bonding strength at the phase interface. In addition, the reinforcing phase is easy to agglomerate, resulting in structural defects such as uneven alloy structure composition and abnormal grain growth. The above problems will lead to a reduction in the mechanical properties of the material. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a nickel-based high-temperature alloy composite material reinforced with nano-ceramic particles. The obtained composite material significantly improves the high-temperature strength, hardness and wear resistance of the material while maintaining the good plasticity of the original material; another purpose of the present invention is to provide a method for preparing the above-mentioned nickel-based high-temperature alloy composite material.
[0005] Technical solution: The nano-ceramic particle reinforced nickel-based high-temperature alloy composite material described in the present invention is a composite material in which TiC nano-ceramic particles and TiB2 nano-ceramic particles are uniformly dispersed in a matrix alloy; during the preparation of the composite material, a prefabricated aluminum-based intermediate alloy is added, and the mass percentage of the prefabricated aluminum-based intermediate alloy is 0.033% to 0.33%; in the prefabricated aluminum-based intermediate alloy, the mass percentage of each substance is: titanium carbide TiC is 10% to 20%, titanium boride TiB2 is 20% to 30%, and the rest is aluminum.
[0006] The aluminum-based master alloy will decompose during the preparation process, and the final organizational state of the material is matrix alloy (nickel-based high-temperature alloy) + TiC, TiB2 (ceramic reinforcement phase).
[0007] The composite material is mixed with the following components in percentage by mass: nickel: 50% to 55%; chromium: 17% to 21%; niobium: 5.0% to 5.5%; titanium: 0.75% to 1.15%; aluminum: 0.3% to 0.7%; molybdenum: 2.8% to 3.3%; carbon: ≤0.08%; manganese ≤0.35%; cobalt ≤1.0%; copper ≤0.3%; magnesium ≤0.01%; silicon ≤0.35%; sulfur ≤0.015%; phosphorus ≤0.015%; aluminum-based master alloy: 0.033% to 0.33%; iron: the rest.
[0008] Among them, the nano ceramic particles are TiC and TiB2, which are added into the alloy smelting process in the form of prefabricated aluminum-based master alloy. The prefabricated aluminum-based master alloy is prepared by the following method, specifically:
[0009] (1) Aluminum powder, titanium powder and boron carbide powder are mixed and placed in a ball mill, and stearic acid is added thereto, wherein the mass of the stearic acid is 1.5-3% of the total mass of the mixed powder, and the ball mill is placed on a ball mill for ball milling, wherein the grinding balls are made of zirconium dioxide, the ball-to-material mass ratio is 10-15:1, the ball milling process is 20-30 hours, and the speed of the ball mill is 50-100 r / min; the ball-milled powder is added to ethanol, and ultrasonically vibrated for 1-4 hours at a frequency of 10-50 kHz to obtain an ethanol suspension, and the ethanol suspension is placed in a drying oven for drying to remove the ethanol solvent, the drying temperature does not exceed 80° C., and the drying time is 1-2 hours to obtain a mixed powder;
[0010] (2) The mixed powder is placed in a vacuum hot pressing furnace mold for hot pressing and synthesis reaction. First, the pressure system is started to gradually pressurize the mixed powder in the mold to 70-80 MPa, the pressure is maintained for 10 minutes, and then the pressure is reduced to 5-10 MPa; the vacuum system is started to reduce the gas pressure in the system to below 1 Pa; the heating system is turned on, and the temperature is heated to 500-550°C at a heating rate of 15-20°C / min, and the temperature is maintained for 30-60 minutes to degas, and then the temperature is continued to be increased at a heating rate of 5-10°C / min. When the furnace temperature display value rises rapidly (the temperature increase indicates that a reaction has occurred, and the reaction can be maintained at this temperature), the temperature is stopped, and the temperature is maintained for 20-30 minutes; the heating system is turned off, and the temperature is reduced to room temperature, the vacuum is broken, the pressure is released, and the intermediate alloy blank is taken out;
[0011] (3) The intermediate alloy blank is crushed into particles.
[0012] The aluminum-based master alloy is in granular form, and the particle diameter does not exceed 1 mm.
[0013] The preparation method of the above nickel-based high-temperature alloy composite material comprises the following steps:
[0014] (1) Vacuum induction melting
[0015] Pre-load the formulated amount of Ni, Cr, Fe, and Mo raw materials into the crucible of the smelting furnace; put the formulated amount of Al, Ti, Nb, and aluminum-based master alloy into the feeder of the furnace; evacuate the smelting chamber to a vacuum degree of less than 5 Pa; start the induction heating power supply, maintain the molten pool temperature at 1550-1650°C, and gradually melt the metal in the crucible until a complete molten pool is formed; after the metal in the crucible is completely melted, electromagnetic stirring is performed for 10-15 minutes;
[0016] The molten pool temperature is adjusted to 1450-1550°C, and the evacuation is performed to a temperature lower than 1 Pa; Nb, Ti, Al, and aluminum-based master alloy are sequentially added to the melt, and after each material is added, the alloy melt is electromagnetically stirred for 5-10 minutes; the smelted alloy is poured under vacuum or under an argon protective atmosphere to form an electrode rod;
[0017] (2) Electroslag remelting
[0018] The electrode rod is melted by the resistance heat generated when the electric current passes through the slag, and the metal droplets pass through the slag layer to reduce the content of various non-metallic impurities, and finally solidify and crystallize to form a cylindrical ingot; the slag temperature is 1250-1350°C, the working current is 2500-3000A, the working voltage is 45-50V, and the slag composition is: 70% CaF2-15% CaO-15% Al2O3; after the electroslag remelting is completed, the ingot is demolded after cooling in the mold for 10-15 minutes, and the demolded ingot is slowly cooled to room temperature;
[0019] (3) Homogenization
[0020] The ingot is slowly heated from room temperature to 1140-1160°C, and the heating rate is controlled at 50-100°C / hour. When the ingot is evenly heated through, it is kept warm for 20 hours. After the ingot is heated, it is directly heated to 1180-1200°C and kept warm for 20 hours, and then taken out and air-cooled. The remelted ingot is homogenized in a vacuum heat treatment furnace to promote the dissolution of the primary phase and eliminate the segregation of alloy elements.
[0021] (4) Forging
[0022] The ingot is heated by a resistance furnace at a temperature of 1000-1050°C. After 150-200 minutes of heat preservation, the ingot is taken out and quickly placed on a fast forging machine for continuous drawing forging. During the forging process, the workpiece temperature shall not be lower than 900°C. The workpiece shall be deformed as evenly as possible along the circumference. The total forging reduction shall not be less than 70%. Air cooling is performed after forging.
[0023] (5) Solution aging
[0024] The temperature of the solution treatment is 950-980°C. After forging, the rods are placed in a resistance furnace and kept warm for 120-140 minutes, then taken out and water-cooled. After the solution treatment, the temperature of the resistance furnace is adjusted to 720°C for aging treatment. The rods are placed in a resistance furnace and kept warm for 10 hours, then cooled to 620°C at 50-55°C / hour, then kept warm for 8 hours, and taken out and air-cooled.
[0025] Among them, in step (1), the power transmission power of alloy smelting is determined by referring to the mass of the smelted alloy and corresponding to 0.1-0.3KW per kilogram of material, and the power transmission power gradually increases with the amount of alloy added.
[0026] Wherein, in step (1), the diameter of the remelted electrode rod is 100 to 120 mm.
[0027] Wherein, in step (2), the diameter of the water-cooled crystallizer is 150-200 mm, and the depth of the slag pool is 80-100 mm.
[0028] In step (2), the slag should be purified to reduce the impurity content, and its average particle size should not be greater than 5 mm. The slag should be baked and dehydrated before use.
[0029] Wherein, in step (4), the cross-sectional size of the alloy ingot after forging is about Φ45mm to Φ60mm.
[0030] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The present invention introduces nano-ceramic particles into the smelting process of high-temperature alloys in the form of intermediate alloys, and successfully prepares nano-ceramic particle-reinforced nickel-based high-temperature alloy composites; without significantly reducing the plasticity of the material, the high-temperature wear resistance of the composite material is greatly improved, and the high-temperature yield and tensile strength are also significantly improved; the present invention not only avoids surface contamination of nano-particles, but also enables the reinforcing phase nano-particles to be evenly dispersed in the matrix, promoting the dispersion strengthening effect; in addition, it can basically maintain the original smelting process and reduce the material preparation cost. (2) Compared with the nickel-based alloy material without intermediate alloy particles, the average grain size of the high-temperature alloy reinforced by nano-ceramic particles after hot working and solid solution aging treatment is 15 to 20 microns, and the grain size is significantly refined. This is because the nano-ceramic particles play a role of heterogeneous nucleation in the melt, increasing the number of nuclei and achieving the effect of fine grain strengthening. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The electrode rod after vacuum induction smelting in Example 1;
[0032] Figure 2 The ingot after electroslag remelting in Example 1;
[0033] Figure 3 A quasi-static tensile test device for Examples 1 to 2 and Comparative Example 1 at a high temperature of 650°C;
[0034] Figure 4 The friction and wear test device of Examples 1 to 2 and Comparative Example 1 at a high temperature of 650°C;
[0035] Figure 5 The metallographic structures of the alloy materials of Example 1 and Comparative Example 1 after solution aging. DETAILED DESCRIPTION
[0036] Example 1
[0037] The composite material is composed of the following components in mass percentage: nickel: 52%; chromium: 18%; niobium: 5.0%; titanium: 0.8%; aluminum: 0.3%; molybdenum: 3.0%; carbon: ≤0.08%; manganese ≤0.35%; cobalt ≤1.0%; copper ≤0.3%; magnesium ≤0.01%; silicon ≤0.35%; sulfur ≤0.015%; phosphorus ≤0.015%; aluminum-based master alloy: 0.05wt%; iron: the rest;
[0038] The mass percentage of each substance in the aluminum-based master alloy is as follows: titanium carbide TiC is 15%, titanium boride TiB2 is 25%, and the rest is aluminum.
[0039] The prefabricated aluminum-based master alloy is prepared by the following method, specifically:
[0040] (1.1) Aluminum powder, titanium powder and boron carbide powder are mixed and placed in a ball mill, and stearic acid is added thereto, the mass of stearic acid being 2% of the total mass of the mixed powder. The ball mill is placed on a ball mill for ball milling, wherein the grinding balls are made of zirconium dioxide, the ball-to-material mass ratio is 10:1, the ball milling process is 20 hours, and the ball mill speed is 80 r / min; the ball-milled powder is added to ethanol, and ultrasonically vibrated for 2 hours at a frequency of 30 kHz to obtain an ethanol suspension, and the ethanol suspension is placed in a drying oven for drying to remove the ethanol solvent, the drying temperature does not exceed 80°C, and the drying time is 2 hours to obtain a mixed powder;
[0041] (1.2) The mixed powder is placed in a vacuum hot pressing furnace mold for hot pressing and synthesis reaction. First, the pressure system is started, and the mixed powder in the mold is gradually pressurized to 70MPa, and the pressure is maintained for 10 minutes, and then the pressure is reduced to 5MPa; the vacuum system is started to reduce the gas pressure in the system to below 1Pa; the heating system is turned on, and the temperature is heated to 500°C at a heating rate of 20°C / min, and the temperature is maintained for 60 minutes to degas, and then the temperature is continued to be increased at a heating rate of 10°C / min. When the furnace temperature display value increases rapidly, the temperature is stopped, and the temperature is maintained at this temperature for 30 minutes; the heating system is turned off, and the temperature is reduced to room temperature, the vacuum is broken, the pressure is released, and the intermediate alloy blank is taken out;
[0042] (1.3) The intermediate alloy blank is crushed into particles with a particle diameter not exceeding 1 mm.
[0043] The method for preparing the composite material comprises the following steps:
[0044] (1) Raw material preparation
[0045] The metal raw materials required for smelting the matrix alloy should be high-purity metal blocks or sheets, and should be weighed according to the formula of the alloy composition; the intermediate alloy is in granular form with a particle diameter not exceeding 1mm; the raw materials should be clean, rust-free and oil-free.
[0046] (2) Vacuum induction melting
[0047] Pre-load the formulated amount of Ni, Cr, Fe, and Mo heavy metal raw materials into the crucible of the smelting furnace; put the formulated amount of Al, Ti, Nb, and aluminum-based master alloy into the feeder of the furnace; start the cooling water system and the vacuum system, evacuate the smelting chamber to make the vacuum degree less than 5Pa; start the induction heating power supply to gradually melt the metal in the crucible until a complete molten pool is formed; the heating power is set at 0.2KW per kilogram of alloy material, and during the smelting process, the power supply is gradually increased according to the amount of alloy added to keep the molten pool temperature within the range of 1600°C; after the metal in the crucible is completely melted, electromagnetic stirring is performed for 12 minutes, then the power is turned off, the melt temperature is measured, a small amount of melt solidification sample is taken, the alloy element content is detected, and the alloy element composition is further adjusted according to the test results until the element composition of the alloy material is qualified;
[0048] Refining the alloy: appropriately reduce the equipment smelting power, adjust the molten pool temperature to 1500°C, and evacuate to less than 1Pa; add Nb, Ti, Al, and aluminum-based master alloy to the melt in sequence, and electromagnetically stir the alloy melt for 8 minutes after each addition of material;
[0049] The smelted alloy is poured under vacuum or argon protective atmosphere to form a remelting electrode rod (with a diameter of 100 mm). A slag blocking device should be set during the alloy pouring process.
[0050] (3) Electroslag remelting
[0051] The electrode rod is melted by the resistance heat generated when electric current passes through the slag, and the molten metal drops pass through the slag layer to reduce the content of various non-metallic impurities, and finally solidify and crystallize to form a cylindrical ingot; the water-cooled crystallizer has a diameter of 150mm, a slag pool depth of 80mm, a slag temperature of 1250℃, a working current of 2500A, a working voltage of 50V, and a slag composition of 70%CaF2-15%CaO-15%Al2O3. The slag should be purified to reduce the impurity content, and its average particle size is not more than 5mm. The slag needs to be baked and dehydrated before use; after the electroslag remelting is completed, the ingot is demolded after cooling in the mold for 12 minutes, and the demolded ingot is slowly cooled to room temperature.
[0052] (4) Homogenization
[0053] The remelted ingot is homogenized in a vacuum heat treatment furnace to promote the dissolution of the primary phase and eliminate the segregation of alloy elements. The ingot is heated to 1150°C using a step heating system. After the ingot is evenly heated through, it is kept warm for 20 hours. After the ingot is heated, it is directly heated to 1180°C and kept warm for another 20 hours, and then taken out for air cooling.
[0054] (5) Forging
[0055] The ingot is heated for forging in a resistance furnace at a temperature of 1020°C. After 150 minutes of heat preservation, the ingot is taken out and quickly placed on a fast forging machine for continuous drawing forging. During the forging process, the workpiece temperature shall not be lower than 900°C, the workpiece shall be deformed as evenly as possible along the circumference, and the total forging reduction shall not be less than 70%. The cross-sectional size of the alloy ingot after forging is about Φ50mm, and it is air-cooled after forging.
[0056] (6) Solution aging treatment
[0057] The solution and aging treatments were carried out in an electric resistance furnace. The solution treatment temperature was 970°C. The forged bars were placed in the furnace and kept warm for 120 minutes, then taken out and water-cooled. After the solution treatment, the temperature of the resistance furnace was adjusted to 720°C for aging treatment. The bars were placed in the resistance furnace and kept warm for 10 hours, then cooled to 620°C at 50°C / hour, then kept warm for 8 hours, and then taken out and air-cooled.
[0058] Example 2
[0059] The composite material is composed of the following components in mass percentage: nickel: 52%; chromium: 18%; niobium: 5.0%; titanium: 0.8%; aluminum: 0.3%; molybdenum: 3.0%; carbon: ≤0.08%; manganese ≤0.35%; cobalt ≤1.0%; copper ≤0.3%; magnesium ≤0.01%; silicon ≤0.35%; sulfur ≤0.015%; phosphorus ≤0.015%; aluminum-based master alloy: 0.1wt%; iron: the rest;
[0060] The mass percentage of each substance in the aluminum-based master alloy is as follows: titanium carbide TiC is 15%, titanium boride TiB2 is 25%, and the rest is aluminum.
[0061] The prefabricated aluminum-based master alloy is prepared by the following method, specifically:
[0062] (1.1) Aluminum powder, titanium powder and boron carbide powder are mixed and placed in a ball mill, and stearic acid is added thereto, the mass of stearic acid being 2% of the total mass of the mixed powder. The ball mill is placed on a ball mill for ball milling, wherein the grinding balls are made of zirconium dioxide, the ball-to-material mass ratio is 10:1, the ball milling process is 20 hours, and the ball mill speed is 80 r / min; the ball-milled powder is added to ethanol, and ultrasonically vibrated for 2 hours at a frequency of 30 kHz to obtain an ethanol suspension, and the ethanol suspension is placed in a drying oven for drying to remove the ethanol solvent, the drying temperature does not exceed 80°C, and the drying time is 2 hours to obtain a mixed powder;
[0063] (1.2) The mixed powder is placed in a vacuum hot pressing furnace mold for hot pressing and synthesis reaction. First, the pressure system is started, and the mixed powder in the mold is gradually pressurized to 70MPa, and the pressure is maintained for 10 minutes, and then the pressure is reduced to 5MPa; the vacuum system is started to reduce the gas pressure in the system to below 1Pa; the heating system is turned on, and the temperature is heated to 500°C at a heating rate of 20°C / min, and the temperature is maintained for 60 minutes to degas, and then the temperature is continued to be increased at a heating rate of 10°C / min. When the furnace temperature display value increases rapidly, the temperature is stopped, and the temperature is maintained at this temperature for 30 minutes; the heating system is turned off, and the temperature is reduced to room temperature, the vacuum is broken, the pressure is released, and the intermediate alloy blank is taken out;
[0064] (1.3) The intermediate alloy blank is crushed into particles with a particle diameter not exceeding 1 mm.
[0065] The method for preparing the composite material comprises the following steps:
[0066] (1) Raw material preparation
[0067] The metal raw materials required for smelting the matrix alloy should be high-purity metal blocks or sheets, and should be weighed according to the formula of the alloy composition; the intermediate alloy is in granular form with a particle diameter not exceeding 1mm; the raw materials should be clean, rust-free and oil-free.
[0068] (2) Vacuum induction melting
[0069] Pre-load the formulated amount of Ni, Cr, Fe, and Mo heavy metal raw materials into the crucible of the smelting furnace; put the formulated amount of Al, Ti, Nb, and aluminum-based master alloy into the feeder of the furnace; start the cooling water system and the vacuum system, evacuate the smelting chamber to make the vacuum degree less than 5Pa; start the induction heating power supply to gradually melt the metal in the crucible until a complete molten pool is formed; the heating power is set at 0.2KW per kilogram of alloy material, and during the smelting process, the power supply is gradually increased according to the amount of alloy added to keep the molten pool temperature within the range of 1600°C; after the metal in the crucible is completely melted, electromagnetic stirring is performed for 12 minutes, then the power is turned off, the melt temperature is measured, a small amount of melt solidification sample is taken, the alloy element content is detected, and the alloy element composition is further adjusted according to the test results until the element composition of the alloy material is qualified;
[0070] Refining the alloy: appropriately reduce the equipment smelting power, adjust the molten pool temperature to 1500°C, and evacuate to less than 1Pa; add Nb, Ti, Al, and aluminum-based master alloy to the melt in sequence, and electromagnetically stir the alloy melt for 8 minutes after each addition of material;
[0071] The smelted alloy is poured under vacuum or argon protective atmosphere to form a remelting electrode rod (with a diameter of 100 mm). A slag blocking device should be set during the alloy pouring process.
[0072] (3) Electroslag remelting
[0073] The electrode rod is melted by the resistance heat generated when electric current passes through the slag, and the molten metal drops pass through the slag layer to reduce the content of various non-metallic impurities, and finally solidify and crystallize to form a cylindrical ingot; the water-cooled crystallizer has a diameter of 150mm, a slag pool depth of 80mm, a slag temperature of 1250℃, a working current of 2500A, a working voltage of 50V, and a slag composition of 70%CaF2-15%CaO-15%Al2O3. The slag should be purified to reduce the impurity content, and its average particle size is not more than 5mm. The slag needs to be baked and dehydrated before use; after the electroslag remelting is completed, the ingot is demolded after cooling in the mold for 12 minutes, and the demolded ingot is slowly cooled to room temperature.
[0074] (4) Homogenization
[0075] The remelted ingot is homogenized in a vacuum heat treatment furnace to promote the dissolution of the primary phase and eliminate the segregation of alloy elements. The ingot is heated to 1150°C using a step heating system. After the ingot is evenly heated through, it is kept warm for 20 hours. After the ingot is heated, it is directly heated to 1180°C and kept warm for another 20 hours, and then taken out for air cooling.
[0076] (5) Forging
[0077] The ingot is heated for forging in a resistance furnace at a temperature of 1020°C. After 150 minutes of heat preservation, the ingot is taken out and quickly placed on a fast forging machine for continuous drawing forging. During the forging process, the workpiece temperature shall not be lower than 900°C, the workpiece shall be deformed as evenly as possible along the circumference, and the total forging reduction shall not be less than 70%. The cross-sectional size of the alloy ingot after forging is about Φ50mm, and it is air-cooled after forging.
[0078] (6) Solution aging treatment
[0079] The solution and aging treatments were carried out in an electric resistance furnace. The solution treatment temperature was 970°C. The forged bars were placed in the furnace and kept warm for 120 minutes, then taken out and water-cooled. After the solution treatment, the temperature of the resistance furnace was adjusted to 720°C for aging treatment. The bars were placed in the resistance furnace and kept warm for 10 hours, then cooled to 620°C at 50°C / hour, then kept warm for 8 hours, and then taken out and air-cooled.
[0080] Example 3
[0081] The composite material is composed of the following components in mass percentage: nickel: 52%; chromium: 18%; niobium: 5.0%; titanium: 0.8%; aluminum: 0.3%; molybdenum: 3.0%; carbon: ≤0.08%; manganese ≤0.35%; cobalt ≤1.0%; copper ≤0.3%; magnesium ≤0.01%; silicon ≤0.35%; sulfur ≤0.015%; phosphorus ≤0.015%; aluminum-based master alloy: 0.15wt%; iron: the rest;
[0082] The mass percentage of each substance in the aluminum-based master alloy is as follows: titanium carbide TiC is 15%, titanium boride TiB2 is 25%, and the rest is aluminum.
[0083] The prefabricated aluminum-based master alloy is prepared by the following method, specifically:
[0084] (1.1) Aluminum powder, titanium powder and boron carbide powder are mixed and placed in a ball mill, and stearic acid is added thereto, the mass of stearic acid being 2% of the total mass of the mixed powder. The ball mill is placed on a ball mill for ball milling, wherein the grinding balls are made of zirconium dioxide, the ball-to-material mass ratio is 10:1, the ball milling process is 20 hours, and the ball mill speed is 80 r / min; the ball-milled powder is added to ethanol, and ultrasonically vibrated for 2 hours at a frequency of 30 kHz to obtain an ethanol suspension, and the ethanol suspension is placed in a drying oven for drying to remove the ethanol solvent, the drying temperature does not exceed 80°C, and the drying time is 2 hours to obtain a mixed powder;
[0085] (1.2) The mixed powder is placed in a vacuum hot pressing furnace mold for hot pressing and synthesis reaction. First, the pressure system is started, and the mixed powder in the mold is gradually pressurized to 70MPa, and the pressure is maintained for 10 minutes, and then the pressure is reduced to 5MPa; the vacuum system is started to reduce the gas pressure in the system to below 1Pa; the heating system is turned on, and the temperature is heated to 500°C at a heating rate of 20°C / min, and the temperature is maintained for 60 minutes to degas, and then the temperature is continued to be increased at a heating rate of 10°C / min. When the furnace temperature display value increases rapidly, the temperature is stopped, and the temperature is maintained at this temperature for 30 minutes; the heating system is turned off, and the temperature is reduced to room temperature, the vacuum is broken, the pressure is released, and the intermediate alloy blank is taken out;
[0086] (1.3) The intermediate alloy blank is crushed into particles with a particle diameter not exceeding 1 mm.
[0087] The method for preparing the composite material comprises the following steps:
[0088] (1) Raw material preparation
[0089] The metal raw materials required for smelting the matrix alloy should be high-purity metal blocks or sheets, and should be weighed according to the formula of the alloy composition; the intermediate alloy is in granular form with a particle diameter not exceeding 1mm; the raw materials should be clean, rust-free and oil-free.
[0090] (2) Vacuum induction melting
[0091] Pre-load the formulated amount of Ni, Cr, Fe, and Mo heavy metal raw materials into the crucible of the smelting furnace; put the formulated amount of Al, Ti, Nb, and aluminum-based master alloy into the feeder of the furnace; start the cooling water system and the vacuum system, evacuate the smelting chamber to make the vacuum degree less than 5Pa; start the induction heating power supply to gradually melt the metal in the crucible until a complete molten pool is formed; the heating power is set at 0.2KW per kilogram of alloy material, and during the smelting process, the power supply is gradually increased according to the amount of alloy added to keep the molten pool temperature within the range of 1600°C; after the metal in the crucible is completely melted, electromagnetic stirring is performed for 12 minutes, then the power is turned off, the melt temperature is measured, a small amount of melt solidification sample is taken, the alloy element content is detected, and the alloy element composition is further adjusted according to the test results until the element composition of the alloy material is qualified;
[0092] Refining the alloy: appropriately reduce the equipment smelting power, adjust the molten pool temperature to 1500°C, and evacuate to less than 1Pa; add Nb, Ti, Al, and aluminum-based master alloy to the melt in sequence, and electromagnetically stir the alloy melt for 8 minutes after each addition of material;
[0093] The smelted alloy is poured under vacuum or argon protective atmosphere to form a remelting electrode rod (with a diameter of 100 mm). A slag blocking device should be set during the alloy pouring process.
[0094] (3) Electroslag remelting
[0095] The electrode rod is melted by the resistance heat generated when electric current passes through the slag, and the molten metal drops pass through the slag layer to reduce the content of various non-metallic impurities, and finally solidify and crystallize to form a cylindrical ingot; the water-cooled crystallizer has a diameter of 150mm, a slag pool depth of 80mm, a slag temperature of 1250℃, a working current of 2500A, a working voltage of 50V, and a slag composition of 70%CaF2-15%CaO-15%Al2O3. The slag should be purified to reduce the impurity content, and its average particle size is not more than 5mm. The slag needs to be baked and dehydrated before use; after the electroslag remelting is completed, the ingot is demolded after cooling in the mold for 12 minutes, and the demolded ingot is slowly cooled to room temperature.
[0096] (4) Homogenization
[0097] The remelted ingot is homogenized in a vacuum heat treatment furnace to promote the dissolution of the primary phase and eliminate the segregation of alloy elements. The ingot is heated to 1150°C using a step heating system. After the ingot is evenly heated through, it is kept warm for 20 hours. After the ingot is heated, it is directly heated to 1180°C and kept warm for another 20 hours, and then taken out for air cooling.
[0098] (5) Forging
[0099] The ingot is heated for forging in a resistance furnace at a temperature of 1020°C. After 150 minutes of heat preservation, the ingot is taken out and quickly placed on a fast forging machine for continuous drawing forging. During the forging process, the workpiece temperature shall not be lower than 900°C, the workpiece shall be deformed as evenly as possible along the circumference, and the total forging reduction shall not be less than 70%. The cross-sectional size of the alloy ingot after forging is about Φ50mm, and it is air-cooled after forging.
[0100] (6) Solution aging treatment
[0101] The solution and aging treatments were carried out in an electric resistance furnace. The solution treatment temperature was 970°C. The forged bars were placed in the furnace and kept warm for 120 minutes, then taken out and water-cooled. After the solution treatment, the temperature of the resistance furnace was adjusted to 720°C for aging treatment. The bars were placed in the resistance furnace and kept warm for 10 hours, then cooled to 620°C at 50°C / hour, then kept warm for 8 hours, and then taken out and air-cooled.
[0102] Comparative Example 1
[0103] The high-temperature alloy matrix material is composed of the following components in mass percentage: nickel: 52%; chromium: 18%; niobium: 5.0%; titanium: 0.8%; aluminum: 0.3%; molybdenum: 3.0%; carbon: ≤0.08%; manganese ≤0.35%; cobalt ≤1.0%; copper ≤0.3%; magnesium ≤0.01%; silicon ≤0.35%; sulfur ≤0.015%; phosphorus ≤0.015%; iron: the rest.
[0104] The method for preparing the above alloy material comprises the following steps:
[0105] (1) Raw material preparation
[0106] The metal raw materials required for base alloy smelting should be high-purity metal blocks or sheets, and should be weighed according to the formula of the alloy composition. The raw materials should be clean, rust-free and oil-free.
[0107] (2) Vacuum induction melting
[0108] Pre-load the formulated amount of Ni, Cr, Fe, and Mo heavy metal raw materials into the crucible of the smelting furnace; put the formulated amount of Al, Ti, and Nb raw materials into the feeder of the furnace; start the cooling water system and the vacuum system, evacuate the smelting chamber, and make the vacuum degree less than 5Pa; start the induction heating power supply to gradually melt the metal in the crucible until a complete molten pool is formed; the heating power is set at 0.2KW per kilogram of alloy material, and during the smelting process, the power supply is gradually increased according to the amount of alloy added to keep the molten pool temperature within the range of 1600℃; after the metal in the crucible is completely melted, electromagnetic stirring is performed for 12 minutes, and then the power is turned off, the melt temperature is measured, a small amount of melt solidification sample is taken, and the alloy element content is detected, and the alloy element composition is further adjusted according to the test results until the element composition of the alloy material is qualified;
[0109] Refining the alloy: appropriately reduce the equipment smelting power, adjust the molten pool temperature to 1500°C, and evacuate to less than 1Pa; add Nb, Ti, and Al raw materials to the melt in sequence, and electromagnetically stir the alloy melt for 8 minutes after each addition of material;
[0110] The smelted alloy is poured under vacuum or argon protective atmosphere to form a remelting electrode rod (with a diameter of 100 mm). A slag blocking device should be set during the alloy pouring process.
[0111] (3) Electroslag remelting
[0112] The blank is melted by the resistance heat generated when electric current passes through the slag, and the molten metal drops pass through the slag layer to reduce the content of various non-metallic impurities, and finally solidify and crystallize to form a cylindrical ingot; the water-cooled crystallizer has a diameter of 150mm, a slag pool depth of 80mm, a slag temperature of 1250℃, a working current of 2500A, a working voltage of 50V, and a slag composition of 70%CaF2-15%CaO-15%Al2O3. The slag should be purified to reduce the impurity content, and its average particle size is not more than 5mm. The slag needs to be baked and dehydrated before use; after the electroslag remelting is completed, the ingot is demolded after cooling in the mold for 12 minutes, and the demolded ingot is slowly cooled to room temperature.
[0113] (4) Homogenization
[0114] The remelted ingot is homogenized in a vacuum heat treatment furnace to promote the dissolution of the primary phase and eliminate the segregation of alloy elements. The ingot is heated to 1150°C using a step heating system. After the ingot is evenly heated through, it is kept warm for 20 hours. After the ingot is heated, it is directly heated to 1180°C and kept warm for another 20 hours, and then taken out for air cooling.
[0115] (5) Forging
[0116] The ingot is heated for forging in a resistance furnace at a temperature of 1020°C. After 150 minutes of heat preservation, the ingot is taken out and quickly placed on a fast forging machine for continuous drawing forging. During the forging process, the workpiece temperature shall not be lower than 900°C, the workpiece shall be deformed as evenly as possible along the circumference, and the total forging reduction shall not be less than 70%. The cross-sectional size of the alloy ingot after forging is about Φ50mm, and it is air-cooled after forging.
[0117] (6) Solution aging treatment
[0118] The solution and aging treatments were carried out in an electric resistance furnace. The solution treatment temperature was 970°C. The forged bars were placed in the furnace and kept warm for 120 minutes, then taken out and water-cooled. After the solution treatment, the temperature of the resistance furnace was adjusted to 720°C for aging treatment. The bars were placed in the resistance furnace and kept warm for 10 hours, then cooled to 620°C at 50°C / hour, then kept warm for 8 hours, and then taken out and air-cooled.
[0119] At 650°C, quasi-static tensile and friction and wear tests were carried out on the high-temperature alloys reinforced with nano-ceramic particles of Examples 1 to 3 after solution aging treatment and the material of Comparative Example 1 without adding nano-ceramic particles. The experimental conditions are as follows: a 300KN universal tensile testing machine was used to test the three groups of samples for high-temperature tensile mechanical properties at 650°C. The loading speed in the elastic section was 0.45mm / min. After the material entered the yield stage, the loading speed was gradually increased to 2.5mm / min until the sample was broken. The high-temperature mechanical tensile test showed that Figure 3 The friction and wear test uses an Al2O3 ceramic ball with a diameter of 10mm as the friction pair, the test force is 10N, the speed is 100r / min, the heating time is 30min to 650℃, the wear time is 30min, and the wear radius is 5mm. The high temperature friction and wear test is shown in Figure 4 The experimental test results are shown in Table 1.
[0120] Table 1 shows the mechanical properties of high temperature alloys of Examples 1 to 3 and Comparative Example 1 at 650°C
[0121]
[0122] It can be seen from Table 1 that the addition of nano-ceramic particles greatly improves the high-temperature wear resistance of the material while maintaining the plasticity of the original material, and the yield strength and tensile strength at high temperatures are also significantly improved.
[0123] Figure 5 A comparison of the metallographic structures of the composite material without nanoparticles and the composite material with 0.05% mass fraction of nanoparticles added after solution aging is given. As shown in the figure, the average grain size of the microstructure of the composite material with 0.05wt% nanoceramic particles added is significantly smaller than the grain size of the alloy material without nanoceramic particles added, which shows that the addition of nanoceramic particles can produce a fine grain strengthening effect, thereby significantly improving the high temperature mechanical properties of the composite material.
Claims
1. A nano-ceramic particle reinforced nickel-based high-temperature alloy composite material, Features: The composite material is a matrix alloy in which TiC nano-ceramic particles and TiB are uniformly dispersed. 2 Nano ceramic particles; in the preparation process of the composite material, a prefabricated aluminum-based master alloy is added, the mass percentage of the prefabricated aluminum-based master alloy is 0.033% to 0.33%; the mass percentage of each substance in the prefabricated aluminum-based master alloy is: titanium carbide TiC is 10% to 20%, titanium boride TiB 2 It is 20% to 30%, and the rest is aluminum.
2. The nano-ceramic particle reinforced nickel-based high-temperature alloy composite material according to claim 1, It is characterized in that The composite material is mixed with the following components in mass percentage: nickel: 50% to 55%; chromium: 17% to 21%; niobium: 5.0% to 5.5%; Titanium: 0.75% to 1.15%; Aluminum: 0.3% to 0.7%; Molybdenum: 2.8%-3.3%; Carbon: ≤0.08%; Manganese ≤0.35%; Cobalt ≤1.0%; Copper ≤0.3%; Magnesium ≤0.01%; Silicon ≤0.35%; Sulfur ≤0.015%; Phosphorus ≤0.015%; Aluminum-based master alloy: 0.033%~0.33%; Iron: the rest.
3. The nano-ceramic particle reinforced nickel-based high-temperature alloy composite material according to claim 1, Features: The prefabricated aluminum-based master alloy is prepared by the following method, specifically: (1.1) Aluminum powder, titanium powder and boron carbide powder are mixed and placed in a ball mill, and stearic acid is added thereto, wherein the mass of the stearic acid is 1.5-3% of the total mass of the mixed powder; the ball-milled powder is added to ethanol, and ultrasonically shaken for 1-4 hours at a frequency of 10-50 kHz to obtain an ethanol suspension, and the ethanol suspension is placed in a drying oven at a drying temperature not exceeding 80° C. for a drying time of 1-2 hours to obtain a mixed powder; (1.2) The mixed powder is loaded into a vacuum hot pressing furnace mold, and the pressure system is first started to gradually pressurize the mixed powder in the mold to 70-80 MPa, and the pressure is maintained for 5-10 minutes, and then the pressure is reduced to 5-10 MPa; then the vacuum system is started to reduce the gas pressure in the system to below 1 Pa; then the heating system is turned on, and the temperature is heated to 500-550°C at a heating rate of 15-20°C / min, and the temperature is maintained for 30-60 minutes to degas, and then the temperature is continued to be increased at a heating rate of 5-10°C / min. When the furnace temperature display value increases rapidly, the temperature is stopped, and the temperature is maintained at this temperature for 20-30 minutes; the heating system is turned off, and the temperature is reduced to room temperature, the vacuum is broken, the pressure is released, and the intermediate alloy blank is taken out; (1.3) The intermediate alloy blank is crushed into particles.
4. The nano-ceramic particle reinforced nickel-based high-temperature alloy composite material according to claim 1, Features: The aluminum-based master alloy is in granular form, and the particle diameter does not exceed 1 mm.
5. The method for preparing the nickel-based high-temperature alloy composite material according to claim 1, It is characterized in that The steps include: (1) Vacuum induction melting Pre-load the formulated amount of Ni, Cr, Fe, and Mo heavy metal raw materials into the crucible of the smelting furnace; put the formulated amount of Al, Ti, Nb, and aluminum-based master alloy into the feeder of the furnace; evacuate the smelting chamber to a vacuum degree of less than 5 Pa; start the induction heating power supply, heat the molten pool to a temperature of 1550-1650°C, and gradually melt the metal in the crucible until a complete molten pool is formed; after the metal in the crucible is completely melted, electromagnetic stirring is performed for 10-15 minutes; The molten pool temperature is adjusted to 1450-1550°C, and the evacuation is performed to a temperature lower than 1 Pa; Nb, Ti, Al, and aluminum-based master alloy are sequentially added to the melt, and after each material is added, the alloy melt is electromagnetically stirred for 5-10 minutes; the smelted alloy is poured under vacuum or under an argon protective atmosphere to form an electrode rod; (2) Electroslag remelting The electrode rod is melted by the resistance heat generated when the current passes through the slag. The metal droplets pass through the slag layer to reduce the content of various non-metallic impurities, and finally solidify and crystallize to form a cylindrical ingot; the slag temperature is 1250-1350℃, the working current is 2500-3000A, the working voltage is 45-50V, and the slag composition is: 70%CaF 2 -15%CaO-15%Al 2 O 3 After the electroslag remelting is completed, the ingot is cooled in the mold for 10 to 15 minutes before demolding. The demolded ingot is slowly cooled to room temperature. (3) Homogenization The ingot is slowly heated from room temperature to 1140-1160°C, and the heating rate is controlled at 50-100°C / hour. When the ingot is evenly heated through, it is kept warm for not less than 20 hours. After the ingot is heated, it is directly heated to 1180-1200°C and kept warm for not less than 20 hours, and then taken out and air-cooled; (4) Forging The ingot is heated by a resistance furnace at a temperature of 1000-1050°C. After 150-200 minutes of heat preservation, the ingot is taken out and quickly placed on a fast forging machine for continuous drawing forging. During the forging process, the workpiece temperature shall not be lower than 900°C, the total forging reduction shall not be lower than 70%, and air cooling shall be performed after forging. (5) Solution aging treatment The temperature of the solution treatment is 950-980°C. After forging, the rods are placed in a resistance furnace and kept warm for 120-140 minutes, then taken out and water-cooled. After the solution treatment, the temperature of the resistance furnace is adjusted to 700-720°C for aging treatment. The rods are placed in a resistance furnace and kept warm for not less than 10 hours, then cooled with the furnace at 50-55°C / hour to 600-620°C, then kept warm for not less than 8 hours, and then taken out and air-cooled.
6. The method for preparing the nickel-based high-temperature alloy composite material according to claim 5, Features: In step (1), the power supply for alloy smelting is determined by referring to the mass of the alloy to be smelted, and is determined at 0.1 to 0.3 kW per kilogram of material. The power supply gradually increases with the amount of alloy added.
7. The method for preparing the nickel-based high-temperature alloy composite material according to claim 5, Features: In step (1), the diameter of the remelted electrode rod is 100 to 120 mm.
8. The method for preparing the nickel-based high-temperature alloy composite material according to claim 5, Features: In step (2), the diameter of the water-cooled crystallizer is 150-200 mm, and the depth of the slag pool is 80-100 mm.
9. The method for preparing the nickel-based high-temperature alloy composite material according to claim 5, Features: In step (2), the average particle size of the slag is not greater than 5 mm.
10. The method for preparing the nickel-based high-temperature alloy composite material according to claim 5, Features: In step (4), the cross-sectional size of the forged alloy ingot is about Φ45 mm to Φ60 mm.