High-crack-arrest super-thick steel plate and production method thereof
Through the design of low-carbon and low alloy composition and specific rolling process, a gauze-resolution thick steel plate with textured ferrite + bainite structure is formed, which solves the problem of insufficient thickness and crack-resolution performance in the prior art, and realizes the Low-cost and efficient crack-resolution performance meets the needs of high strength and toughness in ship construction.
Patent Information
- Application Number
- CN202410951810.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The thickness of existing high-strength steel plates is generally less than 100mm, and the crack-resistance and toughness of -10℃ is insufficient, which cannot meet the safety needs of large-scale ship transportation. The production cost is high, and the low-temperature crack-resistance and lateral impact performance have not been optimized.
Using low-carbon and low alloy composition design and specific rolling process, textured ferrite + bainite structure is formed, and the gauze-resolution and thick steel plates are produced through converter smelting, LF refining, RH vacuum refining and continuous casting processes. From 80 to 120 mm, the texture ratio is greater than 5%, the yield strength of the steel plate core is greater than 400MPa, the low-temperature impact toughness of -40℃ is greater than 200J, and the crack-resistance toughness of -10℃ is greater than 9000N/mm3/2.
It has achieved the production of extra-thick steel plates with low-cost cracking performance, which has reduced production costs, improved welding performance and steel plate cracking performance, and met the demand for high strength and high toughness in ship construction.
Smart Images

Figure CN118910488A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, in particular to an extra-thick steel plate with high crack arrestability and a production method thereof. Background Art
[0002] The field of marine transportation is developing rapidly, and the performance of ship decks plays an important role in the amount of transport equivalent. At present, the main problem in ship transportation is the brittle fracture of hatch coamings and decks. Therefore, the construction and development of ships urgently need thick plate crack arrest steel with high strength, especially high toughness, so as to increase the single transport volume of ships and ensure better safety performance.
[0003] At present, the mainstream high-performance thick plate crack arrest steel in the world is EH40 and EH47 grades, with a thickness of 40 to 100 mm, and the steel plate crack arrest toughness Kca at -10°C ≥ 6000N / mm 3 / 2 This performance has gradually failed to guarantee the safety of large-scale ship transportation. At present, there are two major problems with high-strength and toughness steel plates: the thickness of the steel plate is generally less than 100mm. And the crack arrest toughness at -10℃ is generally no more than 7000N / mm 3 / 2 Therefore, the research and development of thick steel plates with higher crack arrest performance becomes necessary.
[0004] In the prior art, patent CN112522626A discloses a method for producing high-strength steel with low yield ratio by controlling phase change process. By adjusting the proportion of eutectoid ferrite before entering water, the yield ratio of high-strength steel is adjusted, and the yield strength reaches 580MPa. The thickness of the steel plate produced by this patented technology is 30mm, which is difficult to meet the requirements of extra-thick steel plates, and more Ni and Cr elements are added, which increases the production cost, and does not optimize the low-temperature crack arrest toughness and lateral impact performance. Patent CN101619423A discloses a high-toughness, low-yield ratio, easy-to-weld structural steel plate and its manufacturing method. The steel has a yield strength of not less than 510MPa, and is mainly bainite + ferrite structure, wherein the volume fraction of bainite is 55% to 70% and the volume fraction of ferrite is 30% to 45%. This patent adds more Cr elements, has high production costs, and has low-temperature crack arrest toughness and lateral impact performance, and the thickness of the steel plate is unknown. None of the above patents proposes a targeted solution for extra-thick steel plates with high crack arrest performance.
[0005] In view of the above problems, the present invention is proposed. Summary of the invention
[0006] The invention discloses a production method of a high-crack-arresting extra-thick steel plate, aiming to solve the technical problems existing in the prior art.
[0007] The present invention adopts the following technical solutions:
[0008] In one aspect, the present invention provides a method for producing a high-crack-arresting extra-thick steel plate.
[0009] The production method is carried out according to the following steps:
[0010] Raw material preparation step S1: preparing raw materials with the following chemical composition, which contains, by mass%, C: 0.06-0.12%, Si: 0.3-0.4%, Mn: 1.4-1.8%, Al: 0.20-0.40%, Nb: 0.03-0.05%, Ti: 0.02-0.03%, and the rest is Fe and other inevitable impurities;
[0011] Smelting step S2: smelting the raw materials and pre-treating the molten steel, and then performing converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet;
[0012] Rolling step S4: heating, keeping warm, rolling and water cooling the continuous casting billet to room temperature to form a steel plate;
[0013] The steel plate has a microstructure of textured ferrite and bainite, including {112} <110> Texture.
[0014] As a preferred technical solution, the rolling step S4 includes:
[0015] Rough rolling step S41: a step of rough rolling the heated and heat-insulated continuous casting billet;
[0016] Finishing step S42: When the temperature drops to A C3 The following is the process of finishing rolling at 50°C.
[0017] As a preferred technical solution, the thickness of the steel plate after the rough rolling step S41 is 135 to 200 mm.
[0018] As a preferred technical solution, the thickness of the steel plate after the finish rolling step S42 is 80 to 120 mm.
[0019] As a preferred technical solution, in the rolling step S4, the continuous casting billet is heated to 1150°C±30°C, and the holding time is 120 minutes.
[0020] As a preferred technical solution, it also includes a continuous casting billet pretreatment step S3: heating the continuous casting billet to 1150°C to 1200°C, keeping the temperature for more than 120 minutes and rapidly cooling the billet to below 500°C.
[0021] As a preferred technical solution, the steel plate core yield strength as a steel plate characteristic is greater than 400MPa, the low temperature impact toughness of the steel plate core at -40°C is greater than 200J, and the steel plate 10°C crack arrest toughness Kca ≥ 9000N / mm 3 / 2 .
[0022] As a preferred technical solution, the thickness of the continuous casting embryo is ≥300 mm.
[0023] On the other hand, the present invention also provides a high crack arrestability extra thick steel plate, which is produced according to the above-mentioned production method of the high crack arrestability extra thick steel plate.
[0024] As a preferred technical solution, the steel plate {112} <110> Texture ratio >5%.
[0025] The technical solution adopted by the present invention can achieve at least one of the following beneficial effects:
[0026] 1. The present invention obtains a textured ferrite + bainite structure through low-cost alloy design and specific rolling process, wherein {112} <110> Texture ratio>5%, thus obtaining a high-toughness crack arrest steel plate with a thickness of 80-120mm, a core yield strength of the steel plate greater than 400MPa, a core low-temperature impact toughness of -40℃ greater than 200J, and a -10℃ crack arrest toughness Kca≥9000N / mm 3 / 2 , the crack arrest performance of the steel plate is greatly improved by utilizing the characteristics of the texture.
[0027] 2. The steel plate of the present invention has a simple chemical composition, and the production cost is reduced by removing alloy elements such as Ni and Cr. In addition, the low C composition design reduces the segregation phenomenon in the core of the extra-thick plate and improves the welding performance.
[0028] 3. The present invention utilizes Al as a ferrite stabilizing element to promote the formation of ferrite in the early stage of finishing rolling, so that the ferrite is deformed and textured in the later stage of finishing rolling. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments, which constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions explain the present invention and do not constitute improper limitations on the present invention. In the drawings:
[0030] Figure 1 is a flow chart of the production steps of the present invention;
[0031] Figure 2 This is a schematic diagram of the microstructure of Example 1 of the present invention. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. In the description of the present invention, it should be noted that the term "or" is usually used in the sense of including "and / or", unless the content clearly indicates otherwise.
[0033] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The object of the present invention is to provide a high crack arrest performance extra thick steel plate, which can not only meet the performance requirements of shipbuilding materials, but also reduce the production cost of the material.
[0035] In order to achieve the above-mentioned purpose, the present invention proposes an innovative technical solution, including the use of low-carbon and low-alloy composition design and a specific process flow.
[0036] Embodiment 1:
[0037] Reference Figure 1 , this embodiment is produced according to the following steps:
[0038] S1: The chemical composition of this embodiment is, by mass%, C: 0.08%, Si: 0.3%, Mn: 1.4%, Nb: 0.03%, Ti: 0.03%, and the rest is Fe and other inevitable impurities. The required raw materials are prepared using the above chemical composition.
[0039] S2: The raw materials are smelted, and after being pre-treated with molten iron, they are successively subjected to converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet having a thickness of 300 mm.
[0040] S3: pre-treating the continuous casting billet, specifically, heating the continuous casting billet to 1165° C., keeping the temperature for more than 118 minutes, and then accelerating cooling to below 500° C. to obtain a bainite structure with uniform grains.
[0041] S4: The rolling step includes S41 rough rolling step and S42 finishing rolling step. The continuous casting billet is heated to 1148°C, kept warm for 120 minutes, and then rough rolled to 135-200 mm in S41. When the temperature drops to A C3 S42 finishing rolling is performed at a temperature below 50°C (766°C in this embodiment) to finish rolling the steel plate to a thickness between 80 and 120 mm, and then water-cooled to room temperature.
[0042] The production process parameters of this embodiment are shown in the table:
[0043]
[0044] Sampling tests were carried out on the above steel plates, and the mechanical properties test results are shown in the following table:
[0045]
[0046] In the high crack arrestability extra thick steel plate produced through the above production steps, {112} <110> The texture ratio is: 7.3%.
[0047] Embodiment 2:
[0048] This embodiment is produced according to the following steps:
[0049] S1: The chemical composition of this embodiment is, by mass%, C: 0.08%, Si: 0.3%, Mn: 1.4%, Nb: 0.03%, Ti: 0.03%, and the rest is Fe and other inevitable impurities. The required raw materials are prepared using the above chemical composition.
[0050] S2: The raw materials are smelted, and after being pre-treated with molten iron, they are successively subjected to converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet having a thickness of 300 mm.
[0051] S3: pre-treating the continuous casting billet, specifically, heating the continuous casting billet to 1165° C., keeping the temperature for more than 121 minutes, and then accelerating cooling to below 500° C. to obtain a bainite structure with uniform grains.
[0052] S4: The rolling step includes S41 rough rolling step and S42 finishing rolling step. The continuous casting billet is heated to 1160°C, kept warm for 120 minutes, and then rough rolled to 135-200 mm in S41. When the temperature drops to A C3 S42 finishing rolling is performed at a temperature below 50°C (761°C in this embodiment) to finish rolling the steel plate to a thickness between 80 and 120 mm, and then water-cooled to room temperature.
[0053] The production process parameters of this embodiment are shown in the table:
[0054]
[0055] Sampling tests were carried out on the above steel plates, and the mechanical properties test results are shown in the following table:
[0056]
[0057] In the high crack arrestability extra thick steel plate produced through the above production steps, {112} <110> The texture ratio is: 5.9%.
[0058] Embodiment 3:
[0059] This embodiment is produced according to the following steps:
[0060] S1: The chemical composition of this embodiment is, by mass%, C: 0.08%, Si: 0.4%, Mn: 1.8%, Nb: 0.05%, Ti: 0.02%, and the rest is Fe and other inevitable impurities. The required raw materials are prepared using the above chemical composition.
[0061] S2: The raw materials are smelted, and after being pre-treated with molten iron, they are successively subjected to converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet having a thickness of 300 mm.
[0062] S3: pre-treating the continuous casting billet, specifically, heating the continuous casting billet to 1208° C., keeping the temperature for more than 119 minutes, and then accelerating cooling to below 500° C. to obtain a bainite structure with uniform grains.
[0063] S4: The rolling step includes S41 rough rolling step and S42 finishing rolling step. The continuous casting billet is heated to 1176℃, kept warm for 120min, and then rough rolled to 135-200mm in S41. When the temperature drops to A C3 S42 finishing rolling is performed at a temperature below 50°C (765°C in this embodiment), the steel plate is finished rolled to a thickness between 80 and 120 mm, and then water-cooled to room temperature.
[0064] The production process parameters of this embodiment are shown in the table:
[0065]
[0066] Sampling tests were carried out on the above steel plates, and the mechanical properties test results are shown in the following table:
[0067]
[0068] In the high crack arrestability extra thick steel plate produced through the above production steps, {112} <110> The texture ratio is: 9.2%.
[0069] Embodiment 4:
[0070] This embodiment is produced according to the following steps:
[0071] S1: The chemical composition of this embodiment is, by mass%, C: 0.08%, Si: 0.4%, Mn: 1.8%, Nb: 0.05%, Ti: 0.02%, and the rest is Fe and other inevitable impurities. The required raw materials are prepared using the above chemical composition.
[0072] S2: The raw materials are smelted, and after being pre-treated with molten iron, they are successively subjected to converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet having a thickness of 300 mm.
[0073] S3: pre-treating the continuous casting billet, specifically, heating the continuous casting billet to 1206° C., keeping the temperature for more than 123 minutes, and then accelerating cooling to below 500° C. to obtain a bainite structure with uniform grains.
[0074] S4: The rolling step includes S41 rough rolling step and S42 finishing rolling step. The continuous casting billet is heated to 1170℃, kept warm for 120min, and then rough rolled to 135-200mm in S41. When the temperature drops to A C3 S42 finishing rolling is performed at a temperature below 50°C (771°C in this embodiment), the steel plate is finished rolled to a thickness between 80 and 120 mm, and then water-cooled to room temperature.
[0075] The production process parameters of this embodiment are shown in the table:
[0076]
[0077]
[0078] Sampling tests were carried out on the above steel plates, and the mechanical properties test results are shown in the following table:
[0079]
[0080] In the high crack arrestability extra thick steel plate produced through the above production steps, {112} <110> The texture ratio is: 6.3%.
[0081] Embodiment 5:
[0082] This embodiment is produced according to the following steps:
[0083] S1: The chemical composition of this embodiment is, by mass%, C: 0.12%, Si: 0.3%, Mn: 1.8%, Nb: 0.05%, Ti: 0.03%, and the rest is Fe and other inevitable impurities. The required raw materials are prepared using the above chemical composition.
[0084] S2: The raw materials are smelted, and after being pre-treated with molten iron, they are successively subjected to converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet having a thickness of 300 mm.
[0085] S3: pre-treating the continuous casting billet, specifically, heating the continuous casting billet to 1243° C., keeping the temperature for more than 119 minutes, and then accelerating cooling to below 500° C. to obtain a bainite structure with uniform grains.
[0086] S4: The rolling step includes S41 rough rolling step and S42 finishing rolling step. The continuous casting billet is heated to 1142°C, kept warm for 120 minutes, and then rough rolled to 135-200 mm in S41. When the temperature drops to A C3S42 finishing rolling is performed at a temperature below 50°C (760°C in this embodiment) to finish rolling the steel plate to a thickness between 80 and 120 mm, and then water-cooled to room temperature.
[0087] The production process parameters of this embodiment are shown in the table:
[0088]
[0089] Sampling tests were carried out on the above steel plates, and the mechanical properties test results are shown in the following table:
[0090]
[0091] In the high crack arrestability extra thick steel plate produced through the above production steps, {112} <110> The texture ratio is: 5.4%.
[0092] Embodiment 6:
[0093] This embodiment is produced according to the following steps:
[0094] S1: The chemical composition of this embodiment is, by mass%, C: 0.12%, Si: 0.3%, Mn: 1.8%, Nb: 0.05%, Ti: 0.03%, and the rest is Fe and other inevitable impurities. The required raw materials are prepared using the above chemical composition.
[0095] S2: The raw materials are smelted, and after being pre-treated with molten iron, they are successively subjected to converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet having a thickness of 300 mm.
[0096] S3: pre-treating the continuous casting billet, specifically, heating the continuous casting billet to 1244° C., keeping the temperature for more than 123 minutes, and then accelerating cooling to below 500° C. to obtain a bainite structure with uniform grains.
[0097] S4: The rolling step includes S41 rough rolling step and S42 finishing rolling step. The continuous casting billet is heated to 1139°C, kept warm for 120 minutes, and then rough rolled to 135-200 mm in S41. When the temperature drops to A C3 S42 finishing rolling is performed at a temperature below 50°C (758°C in this embodiment) to finish rolling the steel plate to a thickness between 80 and 120 mm, and then water-cooled to room temperature.
[0098] The production process parameters of this embodiment are shown in the table:
[0099]
[0100] Sampling tests were carried out on the above steel plates, and the mechanical properties test results are shown in the following table:
[0101]
[0102] In the high crack arrestability extra thick steel plate produced through the above production steps, {112} <110> The texture ratio is: 7.4%.
[0103] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A method for producing a high crack arrestability extra thick steel plate, characterized in that: The production method is carried out according to the following steps: Raw material preparation step S1: preparing the raw material with the following chemical composition, which contains, by mass%, C: 0.06-0.12%, Si: 0.3-0.4%, Mn: 1.4-1.8%, Al: 0.20-0.40%, Nb: 0.03-0.05%, Ti: 0.02-0.03%, and the rest is Fe and other inevitable impurities; Smelting step S2: smelting the raw materials and pre-treating the molten steel, and then performing converter smelting, LF refining, RH vacuum refining and continuous casting to form a continuous casting billet; Rolling step S4: heating, keeping warm, rolling and water-cooling the continuous casting billet to room temperature to form the steel plate; The steel plate has a microstructure of textured ferrite and bainite, wherein the microstructure includes {112} <110> Texture.
2. The method for producing a high crack arrestability extra thick steel plate according to claim 1, characterized in that: The rolling step S4 includes: Rough rolling step S41: a step of rough rolling the heated and heat-insulated continuous casting billet; Finishing step S42: When the temperature drops to A C3 The following is the process of finishing rolling at 50°C.
3. The method for producing a high crack arrestability extra thick steel plate according to claim 2, characterized in that: The thickness of the steel plate after the rough rolling step S41 is 135-200 mm.
4. The method for producing a high crack arrestability extra thick steel plate according to claim 2, characterized in that: The thickness of the steel plate after the finish rolling step S42 is 80 to 120 mm.
5. The method for producing a high crack arrestability extra thick steel plate according to claim 1, characterized in that: In the rolling step S4, the continuous casting billet is heated to 1150°C±30°C, and the holding time is 120 minutes.
6. The method for producing a high crack arrestability extra thick steel plate according to claim 1, characterized in that: The method further comprises a continuous casting billet pretreatment step S3: heating the continuous casting billet to 1150° C. to 1200° C., keeping the temperature for more than 120 minutes and rapidly cooling the billet to below 500° C.
7. The method for producing a high crack arrestability extra thick steel plate according to any one of claims 1 to 6, characterized in that: As the properties of the steel plate, the yield strength of the steel plate core is greater than 400 MPa, the low-temperature impact toughness of the steel plate core at -40°C is greater than 200 J, and the crack arrest toughness of the steel plate at 10°C Kca is greater than 9000 N / mm 3 / 2 .
8. The method for producing a high crack arrestability extra thick steel plate according to any one of claims 1 to 6, characterized in that: The thickness of the continuous casting embryo is ≥300 mm.
9. A high crack arresting extra thick steel plate, characterized in that: The method for producing a high crack arrestability extra thick steel plate according to any one of claims 1 to 8 is used for production.
10. The high crack arrestability extra thick steel plate according to claim 9, characterized in that: The steel plate {112} <110> Texture ratio >5%.
Citation Information
Patent Citations
High-strength thick steel plate with excellent crack-arrest property and manufacturing method thereof
CN108660389A
Crack-resistant toughness steel plate and preparation method thereof
CN109055856A
500MPa-grade crack arrest steel plate and production method thereof
CN114480809A
High Strength Steel Plate and High Strength Welded Pipe Excellent in Ductile Fracture Characteristic and Methods of Production of Same