Fe-based alloy having excellent amorphous forming ability, and powder and magnetic core produced from Fe-based alloy
The gas injection method of Fe100-a-b-c-d-xSiaBbPcCdMox alloy was solved by the problem of crystal formation caused by slow cooling speed of the gas injection method, high amorphous quality and spherical powder were obtained, and excellent magnetic characteristics were achieved in the magnetic core. and low iron loss.
Patent Information
- Application Number
- CN202410963150.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-23
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
When the existing gas injection method produces metal powder, the cooling rate is slow, resulting in crystalline formation, making it difficult to obtain high amorphous and spherical cleaning powder.
An alloy composed of Fe100-a-b-c-d-xSiaBbPcCdMox was heated to 1000°C to 1500°C by induction, and gas injection was processed under a pressure of 50 bar to 100 bar to prepare amorphous powder, and graded it into a particle size below 45 μm to make a magnetic field. core.
It is realized that even with gas injection method, it is possible to produce high amorphous, spherical, and clean powder, and the magnetic core has excellent magnetic properties and low iron loss.
Smart Images

Figure BDA0004950914210000081 
Figure BDA0004950914210000091 
Figure BDA0004950914210000092
Abstract
Description
Technical Field
[0001] The present invention relates to an Fe-based alloy having excellent amorphous forming ability, and powder and a magnetic core produced from the Fe-based alloy. Background Art
[0002] Recently, electronic, information, and communication equipment are required to have low power consumption and high efficiency. In order to achieve low power consumption and high efficiency, soft magnetic alloys having good soft magnetic properties (low coercive force and high saturation magnetic flux density) are required.
[0003] Among them, amorphous soft magnetic alloys are used as materials for parts used in electronic devices and are widely used in the form of metal powders.
[0004] Common methods for producing such metal powders include a pulverization method for pulverizing solid metal, a wet method based on a chemical method such as precipitation, and a spray method for melting a metal material and then spraying it with a nozzle. Among them, the spray method is mainly used when producing alloy powders other than pure metals. This spray method can be divided into a water spray method using a liquid such as water and a gas spray method using a gas according to the cooling medium used.
[0005] The water jet method uses water as a cooling medium, which has a high cooling rate and can produce highly amorphous powders. However, during the water jet process, oxides are generated on the powder surface due to the reaction between water and the molten metal, so a reduction process is required. In addition, due to the characteristics of the process, irregularly shaped powders are produced.
[0006] On the other hand, the metal powder manufacturing method based on gas atomization usually produces metal powder by spraying an inert gas such as argon or nitrogen at room temperature while making the molten metal flow out through a nozzle. The powder produced by the gas atomization method is different from the powder produced by the water atomization method. By using an inert gas as the spraying medium, a very clean powder can be produced, and the powder shape is also a perfect spherical. However, since the cooling medium is a gas, the cooling speed is usually slower than that of the water atomization method, so there is a problem that the produced powder is slowly cooled and becomes crystalline.
[0007] Therefore, there is a need for an alloy for producing amorphous metal powder having a high degree of amorphism, a spherical shape, and cleanness even by a gas jet method.
[0008] Prior art literature
[0009] Patent Literature
[0010] Korean Patent Gazette No. 10-1426017 (granted on July 28, 2014) Summary of the invention
[0011] The technical solution of the present invention is to provide an Fe-based alloy with excellent amorphous forming ability, and powders and magnetic cores manufactured from the Fe-based alloy.
[0012] However, the technical solution of the present invention is not limited to the above-mentioned technical solutions, and other technical solutions not mentioned can be clearly understood by those skilled in the art from the following description.
[0013] According to one aspect of the present invention, there is provided an Fe-based alloy with excellent amorphous forming ability, which is an alloy having a component formula of Fe 100-a-b-c-d-x Si a B b P c C d Mo x When the component formula satisfies 0 < a ≤ 10, 0 < b ≤ 10, 0 < c ≤ 5, 0 < d ≤ 5, 1 < x < 4, the content of Fe is (100 - a - b - c - d - x) at%, the content of Si is a at%, the content of B is b at%, the content of P is c at%, the content of C is d at%, and the content of Mo is x at%.
[0014] According to another aspect of the present invention, there is provided an amorphous powder, and its preparation method is as follows: the alloy is induction heated to a molten temperature of 1000 °C to 1500 °C and completely melted, and then processed by a gas injection method of injecting gas at a pressure of 50 bar to 100 bar to obtain an amorphous powder with a saturation magnetization of 1.2 T or more.
[0015] According to still another aspect of the present invention, there is provided a magnetic core, which is a magnetic core formed by classifying the amorphous powder to a particle size of 45 μm or less and then pressing it at normal temperature and 1000 Mpa, and the magnetic permeability is 30 μa or more.
[0016] The present invention configured as above can expect the following effects.
[0017] The alloy of the present invention has the effect that powders with excellent amorphous forming ability can be manufactured. Even when manufacturing large-diameter powders by the gas injection method, the degree of amorphousness is still very high.
[0018] In addition, the amorphous powder of the present invention has a high degree of amorphousness and excellent magnetic properties.
[0019] In addition, the magnetic core of the present invention has a high degree of amorphousness and excellent magnetic properties.
[0020] The effects of the present invention are not limited to the above effects, and other effects not mentioned can be clearly understood by those skilled in the art from the description and drawings of this case. Detailed implementation manners
[0021] In the present specification, when it is mentioned that a certain part “includes” a certain constituent element, this means that other constituent elements are not excluded and other constituent elements may be included unless otherwise stated.
[0022] The present invention is described in more detail below.
[0023] According to one embodiment of the present invention, an alloy is provided, which has Fe 100-a-b-c-d-x Si a B b P c C d Mo x The alloy of the composition formula, in the composition formula, satisfies 0 <a≤10、0<b≤10、0<c≤5、0<d≤5、1<x<4。
[0024] In the composition formula of the alloy, the words represented by the subscripts may mean the at% unit content of each element in the alloy. That is, in the alloy, the content of Fe is (100-abcdx) at%, the content of Si is a at%, the content of B is bat%, the content of P is cat%, the content of C is d at%, and the content of Mo is x at%.
[0025] That is, in the alloy of one embodiment of the present invention, the Si content is 10 at % or less, the B content is 10 at % or less, the P content is 5 at % or less, the C content is 5 at % or less, and the Mo content is greater than 1 at % and less than 4 at %.
[0026] In the alloy of one embodiment of the present invention, in the composition formula, 2≤x≤3 may be satisfied. That is, the alloy of one embodiment of the present invention may contain 2at% to 3at% of Mo. When Mo is contained in the content within the range, the alloy has excellent amorphous forming ability. Specifically, the crystallization energy retention rate described later is greater than 90%, and the relative coercive force described later is less than 20, so the amorphous forming ability is excellent.
[0027] The composition formula of the alloy according to one embodiment of the present invention may satisfy 5≤a≤9, 7≤b≤10, 3≤c≤7, and 1≤d≤4. That is, the alloy according to one embodiment of the present invention may contain Si in an amount of 5 to 9 at%, B in an amount of 7 to 10 at%, P in an amount of 3 to 7 at%, and C in an amount of 1 to 4 at%. When Si, B, P, and C are contained in the amounts within the ranges, an effect of being able to form an amorphous phase under high cooling conditions may be achieved.
[0028] The alloy according to one embodiment of the present invention may contain 70 to 90 at % of Fe. When Fe is contained within the above range, basic physical properties of the alloy can be achieved, and in particular, magnetic properties can be ensured when the alloy is used as a magnet.
[0029] The alloy according to one embodiment of the present invention is Fe 73 Si a B b P 5 C 3 Mo x The alloy of the composition formula may satisfy 5≤a≤9, 7≤b≤10, and 2≤x≤3. That is, it may contain Si in an amount of 5at% to 9at%, B in an amount of 7at% to 10at%, and Mo in an amount of 2at% to 3at%.
[0030] When Si, B, and Mo are contained in the above-mentioned content range, the amorphous forming ability of the alloy can be improved, which has the effect of reducing the cooling rate required for amorphous formation.
[0031] Since the alloy according to one embodiment of the present invention is excellent in amorphous formation ability, it has the effect of being able to produce a powder with a high degree of amorphousness even when a large-diameter powder is produced by a gas jet method.
[0032] The term "amorphous forming ability" used in this specification means how well an alloy with a high degree of amorphism can be formed. When an alloy with a relatively high degree of amorphism can be formed under the same conditions, it can be said that the amorphous forming ability is excellent.
[0033] On the other hand, the alloy strip generally has a tendency to have a lower amorphous degree as the thickness increases. As the thickness increases, the cooling rate slows down, so the amorphous degree decreases. Therefore, if the alloy has excellent amorphous forming ability, the amorphous degree will be high not only in the thin strip shape but also in the thick strip shape.
[0034] According to one embodiment of the present invention, the amorphous forming ability can be evaluated by various measurement values. The amorphous forming ability can be compared by comparing the high and low parameters including the physical property measurement values that vary with the amorphous degree, and the parameters of the examples described below can be used. However, it is not limited to the examples listed below.
[0035] As a physical property that changes with the degree of amorphousness, for example, crystallization energy can be used. Crystallization energy is the latent heat energy generated by the crystallization of the amorphous alloy ribbon. The so-called high crystallization energy means that the amorphous alloy ribbon needs to be crystallized more, and the amorphous fraction of the alloy ribbon will be high. For example, the crystallization energy of an alloy with a high amorphous fraction can be about 70 J / g or more. On the contrary, the so-called low crystallization energy means that the amorphous alloy ribbon can be crystallized only slightly, and the amorphous fraction of the alloy ribbon will be low.
[0036] Therefore, in the case of an alloy having excellent amorphous-forming ability, the crystallization energy is high even in a thick ribbon shape.
[0037] In general, the amorphous forming ability can be evaluated by comparing the crystallization energy of a thinner strip-shaped alloy with that of a thicker strip-shaped alloy. Specifically, the amorphous forming ability can be evaluated using the crystallization energy retention rate represented by the following formula 1.
[0038] [Formula 1]
[0039] GFA energy (%) = 100*B / A
[0040] In Formula 1, GFA energy wherein: A is the crystallization energy retention rate, B is the crystallization energy measured by heating the alloy from room temperature to 800°C at a heating rate of 40K / s using a differential scanning calorimeter (DSC), and A is the crystallization energy measured by heating the alloy from room temperature to 800°C at a heating rate of 40K / s using a differential scanning calorimeter (DSC).
[0041] As the crystallization energy retention rate represented by the above formula 1 approaches 100%, a highly amorphous alloy ribbon can be formed even if the thickness increases. The alloy according to one embodiment of the present invention can satisfy the following formula 2.
[0042] [Formula 2]
[0043] 40 <GFA energy <100
[0044] In addition, the alloy according to one embodiment of the present invention may satisfy the following formula 3.
[0045] [Formula 3]
[0046] 90 <GFA energy <100
[0047] In the above formula 2 and formula 3, GFA energy is the crystal energy retention rate.
[0048] That is, the crystallization energy retention rate of the alloy of one embodiment of the present invention is greater than 40%, or greater than 90%. Even if the thickness of the alloy strip increases from 70μm to 120μm, the crystallization energy does not decrease much, the amorphous degree remains unchanged, and the amorphous forming ability is very excellent.
[0049] As a physical property that changes with the degree of amorphism and is used to evaluate the amorphous forming ability of the alloy according to one embodiment of the present invention, for example, coercivity can be used. Generally, the coercivity of an alloy tends to decrease as the degree of amorphism increases.
[0050] That is, the lower the coercivity of the alloy, the higher the amorphous fraction of the alloy. For example, the coercivity of an alloy with a high amorphous fraction may be less than about 10 Oe. Conversely, the higher the coercivity of the alloy, the lower the amorphous fraction of the alloy.
[0051] Therefore, in the case of an alloy having excellent amorphous-forming ability, the coercive force is low even in a thick ribbon shape.
[0052] In general, the ability to form amorphous phase can be evaluated by comparing the coercivity of a thinner strip-shaped alloy with that of a thicker strip-shaped alloy. Specifically, the relative coercivity expressed by the following formula 4 can be used to evaluate the ability to form amorphous phase.
[0053] [Formula 4]
[0054] GFA coercivity (Oe) = C2 / D
[0055] In the above formula 4, GFA coercivity is the relative coercive force, C is the coercive force obtained by making the alloy into a thin strip with a thickness of 120 μm, a width of 2 mm and a length of 2 mm and measuring it using a vibrating sample magnetometer (Hubin Company) under conditions of an applied magnetic field of -15 kOe to 15 kOe, and D is the coercive force obtained by making the alloy into a thin strip with a thickness of 70 μm, a width of 2 mm and a length of 2 mm and measuring it using a vibrating sample magnetometer (Vibrating Sample Magnetometer) under conditions of an applied magnetic field of -15 kOe to 15 kOe.
[0056] The lower the relative coercive force expressed by the above formula 4, the more amorphous alloy strip can be formed even if the thickness becomes thicker. Even if the thickness of the thin strip becomes thicker, the coercive force itself needs to decrease. Therefore, unlike the above formula 1, the relative coercive force is calculated by using the product of the coercive forces in the shape of a thin strip with a thickness of 120μm, so that the amorphous forming ability can be evaluated.
[0057] The alloy according to one embodiment of the present invention may satisfy the following formula 5.
[0058] [Formula 5]
[0059] 0 <GFA coercivity <150
[0060] In addition, the alloy according to one embodiment of the present invention may satisfy the following formula 6.
[0061] [Formula 6]
[0062] 0 <GFA coercivity <20
[0063] In the above equations 5 and 6, GFA coercivity is the relative coercive force.
[0064] That is, the relative coercive force of the alloy of one embodiment of the present invention has a value less than 150Oe, or less than 20Oe, so even if the thickness of the alloy strip increases from 70μm to 120μm, the coercive force does not increase much, the amorphous degree remains unchanged, and the amorphous forming ability is very excellent.
[0065] According to another embodiment of the present invention, an amorphous powder is provided, wherein the alloy is induction heated to a melting temperature of 1000°C to 1500°C and completely melted, and then treated by a gas injection method in which gas is injected at a pressure of 50 bar to 100 bar to produce a powder having a saturation magnetization of 1.2 T or more.
[0066] Although the amorphous powder is produced by the gas jet method, the amorphous degree is still high by using the alloy as a raw material, so that the powder has high sphericity and high amorphous degree.
[0067] The amorphous powder can be produced by treating the melt obtained by induction heating and completely melting the alloy using a gas jet method. The gas jet method can be performed using equipment used in the conventional gas jet method, and the amorphous powder can be produced using the gas jet method in a specific manner as shown in the following example.
[0068] According to one embodiment of the present invention, the amorphous powder can be manufactured by a method comprising the following steps: a step of placing an alloy into a crucible to form a melt; a step of allowing the melt to be discharged from the crucible through a pipe; a step of spraying the discharged melt with a gas to form droplets; and a step of rapidly cooling the droplets to manufacture the amorphous powder.
[0069] Each step is described in detail below.
[0070] First, the alloy of one embodiment of the present invention is put into a crucible to form a melt. In order to melt the alloy, the temperature of the heating crucible can be heated to a temperature above the melting point of the alloy component. At this time, the heating crucible used to form the melt can use an ordinary melt crucible, as long as it can be used at a temperature above the melting point of the alloy, it is not limited thereto.
[0071] In addition, the molten alloy may be formed by heating the alloy to about 1000°C to 1500°C or 1000°C to 1100°C.
[0072] Then, the molten metal is discharged from the crucible through a tube. At this time, the tube is preferably heated to 150° C. to 1600° C. This is to prevent the molten metal from cooling rapidly when the molten metal is discharged through the tube. In addition, the diameter of the tube is preferably 0.5 mm to 5 mm.
[0073] Then, the molten metal is sprayed with gas to form droplets. Specifically, the molten metal is sprayed with high pressure gas through a jet nozzle at a supersonic speed to form droplets.
[0074] As the high-pressure gas, a gas with low reactivity such as an inert gas can be used, and helium, argon, nitrogen, etc. can be used.
[0075] In addition, the pressure of the high-pressure gas may be 20 bar to 300 bar or 50 bar to 100 bar, for example, 80 bar. The high-pressure gas in the pressure range is ejected through a nozzle at a supersonic speed, so that the cooling rate of the melt can be maximized. Therefore, amorphous powder can be produced and the production yield can be improved.
[0076] In addition, the high-pressure gas is preferably supplied at a flow rate of 2 to 4 times the volume of the molten metal ejected through the nozzle.
[0077] Then, the liquid droplets may be rapidly cooled to produce amorphous powder. At this time, the liquid droplets may be rapidly cooled at a rate of 100° C. / sec or more, thereby preventing crystals from being generated inside the powder and producing amorphous powder.
[0078] In addition, the cooling may utilize, but is not limited to, cooling equipment used in conventional gas injection methods.
[0079] According to one embodiment of the present invention, the sphericity of the amorphous powder may be 1.5 or less. The so-called sphericity is used to indicate the ratio of the major axis to the minor axis of the particle. The closer it is to 1, the closer it is to a true sphere. Since the sphericity is 1.5 or less, when the powder is used to manufacture components such as magnetic cores, the filling rate will be high, thereby reducing iron loss and having excellent magnetic properties.
[0080] According to an embodiment of the present invention, the particle size of the amorphous powder may be less than 35 μm. By having a particle size within the above range, the eddy current loss may be reduced when manufacturing a magnetic core.
[0081] According to an embodiment of the present invention, the saturation magnetization of the amorphous powder may be greater than 1.2 T. The amorphous powder may be produced by a gas jet method which is a cheaper process and may not reduce the saturation magnetization.
[0082] According to another embodiment of the present invention, a magnetic core is provided, which is obtained by classifying the amorphous powder into particles with a size of less than 45 μm and then pressurizing the powder at room temperature and 1000 MPa, and has a magnetic permeability of more than 30 μa.
[0083] The magnetic core is manufactured using the powder as a raw material, and thus has a high amorphous degree, and thus has the effects of low iron loss and excellent DC superposition characteristics even at high frequencies.
[0084] According to an embodiment of the present invention, the core has an iron loss of less than 660 mW / cc under the conditions of 100 kHz and 0.1 T, and has excellent low iron loss characteristics.
[0085] The following detailed description is given of the embodiments for the purpose of specifically illustrating the present invention. However, the embodiments of the present invention can be modified into various forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. The embodiments of this specification are provided to more fully illustrate the present invention to those of ordinary skill in the industry.
[0086] Example 1
[0087] Prepare Fe 73 Si 7 B 10 P 5 C 3 Mo 2 After the master alloy of the components (Korea Vacuum Metallurgy), the chamber interior is replaced with Ar, N 2 Or He low-reactivity gas, then melt the alloy by induction heating, inject gas to make soup, at this time, the wheel speed is set to 1000rpm or 300rpm, respectively, to produce alloy strips with a thickness of 70μm or 120μm.
[0088] Example 2 and Comparative Examples 1 to 3
[0089] Alloy ribbons of Example 2 and Comparative Examples 1 to 3 were manufactured in the same manner as in Example 1, except that a mother alloy having the composition shown in Table 1 below was used.
[0090]
Table 1
[0091]
[0092]
[0093] Experimental Example 1: Evaluation of amorphous formation ability by crystallization energy parameters
[0094] 0.1 g of alloy strips with a thickness of 70 μm or 120 μm manufactured in Examples 1 to 2 and Comparative Examples 1 to 3 were loaded on the sample pan of a differential scanning calorimeter (DSC). The temperature was increased at a rate of 0.3°C / s for 1200 seconds in the temperature range of 25°C to 800°C. Two experiments were conducted in the said interval and the DSC curve chart was recorded.
[0095] In the obtained DSC curve graph, the crystallization energy was derived from the height of the highest peak point and is shown in Table 2.
[0096] In addition, the crystallization energy of the alloy ribbon having a thickness of 70 μm or 120 μm was calculated, and the crystallization energy retention rate was calculated according to the following formula 1.
[0097] [Formula 1]
[0098] GFAenergy(%)=100*B / A
[0099] In Formula 1, GFAenergy is the crystallization energy retention rate, B is the crystallization energy measured by heating the alloy manufactured in the embodiment or the comparative example from room temperature to 800°C at a heating rate of 40K / s using a differential scanning calorimeter (DSC), and A is the crystallization energy measured by heating the alloy manufactured in the embodiment or the comparative example from room temperature to 800°C at a heating rate of 40K / s using a differential scanning calorimeter (DSC).
[0100]
Table 2
[0101]
[0102] Referring to Table 2 above, Examples 1 and 2 contain Mo in a content of more than 1 at % and less than 4 at %, and thus it can be confirmed that the amorphous forming ability is very high.
[0103] On the contrary, in Comparative Examples 1 to 3, Mo was not contained or was contained too little or too much, and the alloy ribbon was crystallized even if the ribbon thickness was slightly increased, which confirmed that the amorphous forming ability was very low.
[0104] Experimental Example 2: Evaluation of amorphous formation ability by coercivity parameter
[0105] The alloy strips with a thickness of 70 μm or 120 μm manufactured in Examples 1 to 2 and Comparative Examples 1 to 3 were cut into 2 mm*2 mm sizes and mounted on a vibrating sample magnetometer (VSM, Lakeshore Company). When the alloy strips were vibrated at a frequency of 40 Hz in the range of -15 kOe to 15 kOe, the magnetic moment corresponding to the applied magnetic field measured by the Hall sensor was measured, and the hysteresis curve chart of the alloy strip was obtained.
[0106] Table 3 shows the coercive force data obtained from the distances between the points where the slope of the curve changes sharply in the obtained hysteresis curve graph.
[0107] In addition, the coercive force of the alloy ribbon having a thickness of 70 μm or 120 μm was calculated, and the relative coercive force was calculated according to the following formula 3.
[0108] [Formula 4]
[0109] GFA coercivity (Oe) = C2 / D
[0110] In the above formula 4, GFA coercivity is the relative coercive force, C is the coercive force of the alloy strip with a thickness of 120 μm manufactured in the examples or comparative examples, and D is the coercive force of the alloy strip with a thickness of 70 μm manufactured in the examples or comparative examples.
[0111]
Table 3
[0112] 70μm Coercivity(Oe) 120μm Coercivity(Oe) Relative coercivity (Oe) Comparative Example 1 9.91 227.04 5201 Example 1 7.67 10.84 15.32 Example 2 6.69 6.70 6.71 Comparative Example 2 97.81 100.95 104.19 Comparative Example 3 8.17 193.83 4598
[0113] Referring to Table 3, the amorphous phase forming ability values of Examples 1 and 2 are less than 20 Oe, which confirms that the coercive force is low even when the ribbon thickness increases, and thus the amorphous phase forming ability is high.
[0114] On the contrary, in the case of Comparative Example 2, Mo was excessively contained, and when the ribbon thickness increased, the alloy ribbon crystallized and the coercivity increased, thereby confirming that the amorphous forming ability was low. In particular, in the cases of Comparative Examples 1 and 3, Mo was not contained or contained too little, and even if the ribbon thickness was slightly increased, the alloy ribbon crystallized and the coercivity increased significantly, thereby confirming that the amorphous forming ability was very low.
[0115] Experimental Example 3: Crystallinity Analysis by XRD Pattern
[0116] The alloy ribbons of Example 2 and Comparative Examples 2 to 3 were subjected to XRD analysis using an X-ray diffractometer (Rigaku D / Max-2500VL / PC) at 2θ=30 to 70°.
[0117] It can be confirmed that the Mo-containing alloy strips of Example 2 and Comparative Example 2 do not show peaks corresponding to the crystalline phase at a thickness of 70 μm and 120 μm, and a wide halo spectrum is shown near 40 to 50° in the XRD spectrum of the typical amorphous phase, while the alloy strip of Comparative Example 3, as thicker as it is, will clearly show crystalline phase peaks corresponding to FexB and Fe(Si). The higher the corresponding peak is observed, the higher the crystallinity can be considered. That is, it can be confirmed that the alloy strip of Comparative Example 3 has a crystalline internal structure under the condition of a thicker thickness of 120 μm, and it can be known that the component of Example 2 containing Mo still maintains an amorphous phase under the conditions of thickening the thin strip and decreasing the cooling rate, and is a component with high amorphous formation ability.
[0118] Example 3: Preparation of powder
[0119] Based on the alloy composition manufactured in Example 2, 25 kg of master alloy was prepared by induction melting method and put into a batch processor. The molten metal at the lower end of the batch processor was maintained at 1000°C to 1100°C, and argon gas was sprayed under the conditions of a nozzle diameter of 2.5 mm and a pressure of 80 bar, thereby producing amorphous powder.
[0120] Reference example 1
[0121] As a commercially available powder, Kuamet 6B2 powder (particle size <45 μm, saturation magnetization 1.22 T) from Epson Atmix was prepared.
[0122] Experimental Example 4: Evaluation of Powder Properties
[0123] Powder SEM image confirmation
[0124] Using a field emission scanning electron microscope (FE-SEM, MIRA3 LM), a scanning electron microscope (SEM) image of the powder produced in Example 3 was taken at a magnification of 5000 under an applied voltage of 15 kV, and it was confirmed that the formed powder particles were spherical.
[0125] Particle size analysis of powders
[0126] A graph showing the volume occupied by each particle size of the powder produced in Example 3.
[0127] In addition, the value obtained by dividing the major axis length of the powder by the minor axis length, ie, the sphericity of the powder, was calculated by SEM image analysis.
[0128] Referring to the SEM image analysis, it can be confirmed that about 80% of the powder produced in Example 3 has a particle size of about 10 μm to 50 μm, and the average particle size (D50) is about 27.49 μm.
[0129] XRD analysis of powder
[0130] The XRD pattern of the powder prepared in Example 3 was derived using an X-ray diffractometer (D / Max-2500VL / PC manufactured by Rigaku Corporation, Japan) at 2θ=30-70°.
[0131] The powder produced in Example 3 showed a broad halo pattern and no peak corresponding to crystallization appeared, so it was confirmed to be a typical amorphous phase.
[0132] Evaluation of the magnetic properties of powders
[0133] 0.1 g of the powder of Example 3 and Reference Example 1 was loaded into a vibrating sample magnetometer (VSM, Lakeshore). When vibration was applied to the alloy strip at a frequency of 40 Hz in the range of -15 kOe to 15 kOe, the magnetic moment corresponding to the applied magnetic field measured by the Hall sensor was measured, and the hysteresis curve chart of the alloy powder was obtained.
[0134] The hysteresis curve graphs of the powders of Example 3 and Reference Example 1 are shown.
[0135] In addition, data of coercive force, saturation magnetic moment, and saturation magnetization were obtained from the hysteresis curve graph and are shown in Table 4.
[0136]
Table 4
[0137] Coercivity(Oe) Saturation magnetic moment (emu / g) Saturation magnetization (T) Example 3 7.669 128.15 1.21 Reference example 1 7.383 139.01 1.22
[0138] Referring to Table 4 above, the powder of Example 3 exhibits a saturation magnetization level similar to that of the commercially available powder, i.e., the powder of Reference Example 1, and can also be applied to a common gas injection process, thus having the advantage of low powder price.
[0139] Example 4: Manufacturing of magnetic core
[0140] The powder produced in Example 3 was sieved to less than 45 μm, mixed with 1 wt% to 2 wt% of an organic binder, pressed at 80 t at room temperature using a uniaxial press, and cured at 150° C. to produce a magnetic core.
[0141] Reference example 2
[0142] The commercially available powder was sieved to less than 45 μm, mixed with 1 wt% to 2 wt% of an organic binder, pressed at 80 t using a uniaxial press at room temperature, and cured at 150°C to produce a magnetic core.
[0143] Experimental Example 5: Evaluation of magnetic core characteristics
[0144] Evaluation of magnetic core permeability
[0145] Only the primary winding was applied to the manufactured magnetic core, and the magnetic permeability of the magnetic core manufactured in Example 4 and the magnetic core of Reference Example 2 was evaluated at a frequency of 100 Hz to 1 MHz using an LCR meter (Wenco Electronic Instrument Co., Ltd., 3265B).
[0146] The magnetic core manufactured in Example 4 exhibits a higher magnetic permeability than the magnetic core manufactured in Reference Example 2. This is because the powder manufactured using the spinning water atomization (SWAP) method cannot have a perfect sphere, while the powder manufactured using the gas injection method is close to a sphere and has a higher filling rate under the same molding conditions.
[0147] Core loss evaluation
[0148] The primary winding and the secondary winding were wound on the magnetic cores manufactured in Example 4 and Reference Example 2, and the iron loss of the magnetic core was measured by measuring the current induced in the secondary winding while current was connected to the primary winding using a BH analyzer (IWATSU SY-8219).
[0149] The core losses of the magnetic cores manufactured in Example 4 and Reference Example 2 at Bm=0.1T and corresponding to the frequencies are shown in a logarithmic exponential graph.
[0150] It can be confirmed that the iron loss of the magnetic core manufactured in Example 4 is lower than that of the magnetic core manufactured in Reference Example 2.
Claims
1. An Fe alloy having excellent amorphous forming ability, It is characterized in that For Fe 100-a-b-c-d-x Si a B b P c C d Mo x An alloy of components, wherein In terms of the components, <a≤10、0<b≤10、0<c≤5、0<d≤5、1<x<4, The Fe content is (100-abcdx) at%, the Si content is a at%, the B content is b at%, the P content is cat%, the C content is d at%, and the Mo content is x at%.
2. The Fe-based alloy having excellent amorphous forming ability according to claim 1, It is characterized in that in, The following equations 1 and 2 are satisfied: [Formula 1] GFA energy (%)=100*B / A [Formula 2] 40<GFA energy <100 In Formula 1 and Formula 2, GFA energy is the crystal energy retention rate, B is the crystallization energy measured by heating the alloy into a 120 μm thick, 2 mm wide, and 2 mm long thin strip from room temperature to 800° C. at a heating rate of 40 K / s using a differential scanning calorimeter, A is the crystallization energy measured by heating the alloy from room temperature to 800° C. at a heating rate of 40 K / s using a differential scanning calorimeter after forming the alloy into a thin strip with a thickness of 70 μm, a width of 2 mm, and a length of 2 mm.
3. An amorphous powder, It is characterized in that The preparation method is as follows: the Fe alloy with excellent amorphous forming ability as described in claim 1 or 2 is induction heated to a melting temperature of 1000°C to 1500°C to be completely melted, and then treated by a gas injection method of injecting gas at a pressure of 50 bar to 100 bar to obtain an amorphous powder with a saturation magnetization of more than 1.2T.
4. A magnetic core, It is characterized in that The magnetic core is made by classifying the amorphous powder of claim 3 into a particle size of 45 μm or less and then pressurizing it at room temperature and 1000 MPa, and the magnetic permeability is above 30 μa.