Laminated iron core

By optimizing the hardness and sol composition of the insulating coating in the laminated core, combined with the specific chemical composition and texture of the electromagnetic steel plate, the problem of taking into account both the bonding strength and the magnetic characteristics is solved, and the stacking of high bonding strength and excellent magnetic characteristics is achieved Iron core.

CN118974855APending Publication Date: 2024-11-15NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032084.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-04-04
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the laminated core, high bond strength and excellent magnetic properties are difficult to take into account both high bond strength and excellent magnetic properties, and there are problems of deterioration of magnetic properties.

Method used

By controlling the hardness to 200 to 300MPa in the insulating coating, setting the weight average molecular weight of the sol component in the range of 10,000 to 100,000, combined with the specific chemical composition and texture of the electromagnetic steel plate, the hardness and SEM-EBSD are measured using a nano-indenter. The technology determines the grain orientation and optimizes the composition and structure of the insulating coating.

Benefits of technology

The balance between high bonding strength and excellent magnetic characteristics is achieved, the deterioration of magnetic characteristics is suppressed, and a laminated iron core with high bonding strength and excellent magnetic characteristics is provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974855A_ABST
    Figure CN118974855A_ABST
Patent Text Reader

Abstract

This laminated iron core is provided with: a plurality of electromagnetic steel sheets laminated with each other; and an insulating coating film which is provided between the electromagnetic steel sheets adjacent to each other in the lamination direction and which adheres the electromagnetic steel sheets to each other, the insulating coating film having a hardness of 200-300 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated core.

[0002] This application claims priority based on Japanese Patent Application No. 2022-063474 filed in Japan on April 6, 2022, the contents of which are incorporated herein by reference. Background Art

[0003] As an iron core (iron core) for a rotating electric machine, a laminated iron core is known in which a plurality of electromagnetic steel sheets are joined and stacked. As a method for joining the electromagnetic steel sheets, riveting or welding is known. However, during riveting or welding, the magnetic properties of the electromagnetic steel sheets may deteriorate due to mechanical stress or thermal stress during processing and interlayer short circuit, thereby reducing the performance of the laminated iron core.

[0004] Therefore, in recent years, bonding methods have attracted attention as bonding methods other than riveting and welding. Since bonding using an adhesive does not require processing of the steel plate as in riveting, deterioration of magnetic properties can be suppressed in a laminated core (bonded laminated core) formed by stacking and bonding.

[0005] As an adhesive for bonding electromagnetic steel sheets to each other, for example, as disclosed in Patent Document 1, epoxy resins are known that have little volume change and are excellent in heat resistance, oil resistance, and chemical resistance.

[0006] On the other hand, a relatively high temperature is required to cure epoxy resin, so stress is applied to the steel plate during bonding, which may deteriorate the iron loss. Therefore, for example, in Patent Documents 2 to 7, adhesives using polyurethane resins are proposed as adhesives that can be bonded at a lower temperature than epoxy resins.

[0007] Prior Art Literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2022-000888

[0010] Patent Document 2: Japanese Patent Application Publication No. 2017-179233

[0011] Patent Document 3: Japanese Patent Application Publication No. 2017-186542

[0012] Patent Document 4: Japanese Patent Application Laid-Open No. 6-182929

[0013] Patent Document 5: Japanese Patent Application Laid-Open No. 6-271834

[0014] Patent Document 6: Japanese Patent Application Laid-Open No. 7-268051

[0015] Patent Document 7: Japanese Patent Application Publication No. 2002-293864 Summary of the invention

[0016] Technical problem to be solved by the invention

[0017] However, it is known that when such adhesives are used, generally, the higher the adhesive strength, the harder the resin is, and the steel sheet is strained due to curing shrinkage, which deteriorates the magnetic properties. In other words, it is believed that the adhesive strength and the magnetic properties have opposite effects.

[0018] Therefore, conventionally, it has been difficult to achieve both high bonding strength and excellent magnetic properties in bonded laminated cores.

[0019] Therefore, an object of the present invention is to provide a laminated iron core (bonded laminated iron core) having high bonding strength and excellent magnetic properties.

[0020] Technical means for solving technical problems

[0021] The present inventors have studied a method for achieving both high bonding strength and excellent magnetic properties in a laminated core formed by laminating a plurality of electromagnetic steel sheets via an insulating film having bonding ability.

[0022] As a result, it was found that both high adhesive strength and excellent magnetic properties can be achieved in the insulating film by controlling the hardness of the insulating film at the μm level measured by a nanoindenter.

[0023] In addition, the inventors have found that the balance between suppression of magnetic property degradation and improvement of adhesive strength is further improved by setting the weight average molecular weight of the sol component of the insulating coating to a predetermined range.

[0024] The present invention has been accomplished based on the above findings. The gist of the present invention is as follows.

[0025] [1] A laminated iron core according to one embodiment of the present invention comprises a plurality of electromagnetic steel sheets stacked on each other and an insulating coating, wherein the insulating coating is provided between the electromagnetic steel sheets adjacent to each other in a stacking direction, and the electromagnetic steel sheets are bonded to each other, and the hardness of the insulating coating is 200 to 300 MPa.

[0026] [2] In the laminated iron core described in [1], the weight average molecular weight of the sol component of the insulating coating may be 10,000 to 100,000.

[0027] [3] The laminated core according to [1] or [2], wherein among the plurality of electromagnetic steel sheets, when {hkl} is measured by SEM-EBSD on a surface parallel to the rolling surface at a depth of 1 / 2 the sheet thickness from the surface <uvw>When the area ratio of oriented grains to the entire field of view is represented by Ahkl-uvw, A411-011 can also be 15.0% or more.

[0028] [4] The laminated iron core according to any one of [3], wherein the chemical composition of the electromagnetic steel sheet may include, in mass%, C: 0.0100% or less, Si: 1.50% to 4.00%, sol.Al: 0.0001% to 1.0000%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: the total is 0.0000% to 0.0100%, and when the Mn content in mass% is represented as [Mn], the Ni content is represented as [Ni], the Cu content is represented as [Cu], the Si content is represented as [Si], the sol.Al content is represented as [sol.Al], and the P content is represented as [P], the following formula (1) is satisfied: (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol.Al]+4×[P])≧1.50%…(1), and the remainder may also be composed of Fe and impurities.

[0029] Effects of the Invention

[0030] According to the above aspect of the present invention, it is possible to provide a laminated core having high bonding strength and excellent magnetic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a diagram showing an example of a side view of the laminated iron core according to the present embodiment. DETAILED DESCRIPTION

[0032] A laminated core according to one embodiment of the present invention (laminated core according to this embodiment) is as follows Figure 1 As shown, it includes a plurality of electromagnetic steel sheets 21 stacked on each other and an insulating film 22, wherein the insulating film 22 is provided between the electromagnetic steel sheets 21, 21 adjacent to each other in the stacking direction to bond the electromagnetic steel sheets 21, 21 to each other, and the hardness of the insulating film is 200 to 300 MPa.

[0033] The following will explain each one separately.

[0034] <Insulation coating>

[0035] [hardness]

[0036] The insulating film 22 included in the laminated core 1 of the present embodiment ensures insulation and joins the electromagnetic steel sheets 21 , 21 adjacent to each other in the lamination direction by bonding.

[0037] The insulating film is an insulating film with heat-curable adhesiveness when it is formed on the surface of the electromagnetic steel sheet (sometimes referred to as the base steel sheet because it does not have the insulating film). By forming the insulating film with adhesiveness on the base steel sheet, stacking a plurality of electromagnetic steel sheets with the insulating film, and performing heat compression bonding, the electromagnetic steel sheets are bonded by bonding.

[0038] In this case, generally speaking, the higher the bonding strength, the harder the resin, and the shrinkage accompanying the curing imparts strain to the steel sheet, causing the magnetic properties to deteriorate. Therefore, it is not easy to achieve both high bonding strength and excellent magnetic properties at a high level.

[0039] In the laminated core 1 of the present embodiment, the hardness of the insulating film 22 measured by a nanoindenter is controlled to a μm level, thereby suppressing the degradation of magnetic properties and improving the bonding strength. Specifically, the hardness of the insulating film is set to 200 to 300 MPa.

[0040] When the hardness of the insulating film is less than 200 MPa, sufficient bonding strength (for example, 10.0 MPa or more) cannot be obtained. On the other hand, when the hardness of the insulating film exceeds 300 MPa, the magnetic properties deteriorate significantly.

[0041] The hardness of the insulating film can be determined as follows.

[0042] For example, a sample is taken out by cutting out a laminated core from which several pieces have been peeled off with a precision cutter so that the cross section of the insulating film can be observed. A sample for measurement is prepared by performing CP processing (ion milling) on ​​the central portion of the thickness direction of the heated and crimped portion of the insulating film of the sample. The hardness is measured at room temperature (25°C) with a load of 250 μN using a TRIBOINDENTER manufactured by HYSITRON or an equivalent nanoindenter. The measurement is performed at 5 points, and the average value is taken as the hardness of the insulating film.

[0043] [Weight average molecular weight of sol component]

[0044] In the insulating film 22 of the laminated core 1 of the present embodiment, the weight average molecular weight (Mw) of the sol component of the insulating film is preferably 10,000 to 100,000. By setting the weight average molecular weight of the sol component to 10,000 or more, a rigid resin structure can be obtained and sufficient bonding strength can be obtained. In addition, by setting the weight average molecular weight of the sol component to 100,000 or less, the resin does not become too hard, and the degradation of the magnetic properties can be suppressed. That is, by setting the weight average molecular weight of the sol component to a predetermined range, the balance between the suppression of magnetic property degradation and the improvement of bonding strength is further improved.

[0045] The weight average molecular weight of the sol component of the insulating coating is more preferably 20,000 to 70,000, and further preferably 30,000 to 50,000.

[0046] Here, the reason why the weight average molecular weight of the sol component is specified rather than the weight average molecular weight of the entire insulating coating is because the weight average molecular weight of the uncrosslinked portion of the binder affects the magnetic properties.

[0047] The weight average molecular weight of the sol component of the insulating coating can be measured, for example, by using a GPC (Gel Permeation Chromatography) such as a high-speed GPC system HLC-8320GPC manufactured by Toyo Soda, by immersing a cured insulating coating (functioning as an adhesive) cut out from a laminated iron core from which several sheets have been peeled off with a precision cutter in 10 mM lithium bromide-containing N,N-dimethylformamide for 24 hours to prepare a measurement sample. The conditions at this time are as follows.

[0048] Column: PLgel 5μm Guard, PLgel 5μm MIXED-C×2 (Polymer Laboratories)

[0049] Mobile phase: 10 mM N,N-dimethylformamide containing lithium bromide

[0050] Flow rate: 1.0mL / min

[0051] Column temperature: 40°C

[0052] Data processing: EcoSEC-WorkStation

[0053] The insulating film preferably contains 90% by weight or more of an acrylic resin which has a certain degree of rigidity after curing to ensure bonding strength and has low compressive stress on the steel plate due to curing.

[0054] As other components, resins, inorganic salts, and inorganic particles may also be contained. Examples of resins as other components include epoxy resins, polyurethane resins, and phenolic resins. Examples of inorganic salts include phosphates, chromates, and borates. Examples of inorganic particles include silicon dioxide, titanium oxide, magnesium oxide, and zirconium hydroxide. The type of acrylic resin that mainly constitutes the insulating coating is not particularly limited.

[0055] In the laminated core of the present embodiment, another insulating film may be provided as a base layer between the electromagnetic steel sheets 21 and the insulating film 22. In this case, the insulating film bonds the electromagnetic steel sheets to each other via the base layer.

[0056] The base layer is not limited, and a known coating can be used. However, in order to improve insulation and avoid reduction in adhesive strength, a coating formed by applying a general treatment agent such as a chromate treatment agent or a phosphate treatment agent and sintering is preferred.

[0057] The base layer helps to improve the insulation between the stacked steel plates in the core. In order to achieve this effect, the film thickness is preferably set to 0.1 μm or more. On the other hand, if the base layer is thicker, the adhesion is reduced and it is easy to peel off. Therefore, the thickness of the base layer is preferably 1.0 μm or less.

[0058] If the insulating film is too thick, the deterioration of magnetic properties due to the stress of curing increases, while if it is too thin, the bonding area is significantly reduced due to the influence of the surface roughness of the electromagnetic steel sheet to be bonded, and there is a concern that the bonding strength is insufficient.

[0059] Therefore, when the thickness of the bonding portion is represented by A in μm, it is preferred that A and the arithmetic mean roughness Ra of the surface of the electromagnetic steel sheet to be bonded as specified in JIS B0601 (2013) satisfy the following formula (3):

[0060] 3.0×Ra≦A≦3.0(3).

[0061] The thickness A of the insulating film can be measured, for example, by a magnetic method described in JIS K5600-1-7 (2014) using an electromagnetic film thickness meter LE-370 manufactured by Kett Scientific Laboratory or an equivalent electromagnetic film thickness meter.

[0062] In addition, the arithmetic mean roughness Ra of the surface of the electromagnetic steel sheet can be measured using, for example, a surface roughness measuring machine SE3500 manufactured by Kosaka Laboratory or an equivalent stylus type roughness meter. At this time, the measuring direction is set to the sheet width direction (C direction), the measuring length is set to 8 mm, the speed is set to 0.1 mm / s, and the cutoff value is set to 0.8 mm.

[0063] When measuring the arithmetic mean roughness of the surface of the electromagnetic steel sheet when an insulating film or a base layer exists on the surface of the electromagnetic steel sheet, for example after forming a laminated core, the measurement may be performed after removing the insulating film or the base layer from the surface of the electromagnetic steel sheet.

[0064] The insulating coating can be removed by, for example, immersing in DMF (dimethylformamide) for 10 to 60 minutes. The base layer can be removed by, for example, immersing in a 20% NaOH aqueous solution for 1 to 10 minutes.

[0065] <Electromagnetic steel sheet>

[0066] The electromagnetic steel sheets included in the laminated core 1 of the present embodiment may be known electromagnetic steel sheets (oriented electromagnetic steel sheets or non-oriented electromagnetic steel sheets). When application to motors or the like is envisioned, non-oriented electromagnetic steel sheets are preferred.

[0067] Moreover, in the case of a non-oriented electrical steel sheet, it is preferable to have the following texture and chemical composition.

[0068] [Texture]

[0069] In electromagnetic steel sheets, the texture is controlled to obtain low iron loss and high magnetic flux density. For example, the magnetic properties are improved by having an easy magnetization axis within the steel sheet surface, and the development of the aggregated structure (α fibers) can be easily improved by hot rolling and cold rolling, which are necessary steps in the manufacture of steel sheets, thereby improving the magnetic properties. Specifically, the texture is formed <110> A structure oriented substantially parallel to the rolling direction (RD) is effective.

[0070] On the other hand, {100} <011> The change in magnetic properties due to orientation with respect to stress, specifically, the deterioration of magnetic properties when compressive stress acts (stress sensitivity) increases.

[0071] In contrast, by making {411} <011> With the development of this special orientation, the magnetic properties (especially the magnetic properties in the direction 45° from the rolling direction) are further improved.

[0072] Therefore, it is preferable to control the texture, which is the texture measured by a scanning electron microscope with electron backscatter diffraction function (SEM-EBSD) on a surface parallel to the rolling surface at a depth of 1 / 2 of the plate thickness from the surface. <uvw>The area ratio of the grains with a 10° tolerance relative to the entire field of view is denoted as Ahkl-uvw. A411-011 (hereinafter sometimes referred to as {411} <011> The rate) is set to 15.0% or more.

[0073] {411} <011> The rate is more preferably 25.0% or more, further preferably 30.0% or more, further preferably 35.0% or more, and particularly preferably 40.0% or more. The upper limit is not particularly limited, but may be 80.0% or less from the viewpoint of production load.

[0074] The area ratio of specific orientation grains can be measured by the following method. That is, the area ratio of specific orientation grains is determined by using OIM Analysis 7.3 (manufactured by TSL) to extract the specific orientation as the target from the measurement area of ​​a scanning electron microscope (SEM: Scanning Electron Microscope) with electron backscatter diffraction (EBSD: Electron Back Scattering Diffraction) function observed under the following measurement conditions (the tolerance is set to 10°, hereinafter referred to as margin within 10°). The extracted area is divided by the area of ​​the measurement area to obtain the percentage. The percentage is used as the area ratio of specific orientation grains.

[0075] In this embodiment, sometimes "having {hkl} <uvw>The "area ratio of grains with {hkl} orientation (within a tolerance of 10°) relative to the measurement area" and "area ratio of grains with {hkl} orientation (within a tolerance of 10°) relative to the measurement area" are respectively referred to as "{hkl} <uvw>"Rate", "{hkl} rate". In the description of crystal orientation, the margin is within 10°.

[0076] The details of the measurement conditions for obtaining the area ratio of each oriented grain are as follows.

[0077] · Measurement equipment: SEM model "JSM-6400 (manufactured by JEOL)", EBSD detector model "HIKARI (manufactured by TSL)", or similar equipment

[0078] Step interval: 5.0μm

[0079] · Magnification: 100 times

[0080] ·Measurement object: The surface parallel to the rolled surface at a depth of 1 / 2 of the plate thickness from the surface

[0081] ·Measurement area: Rectangular area of ​​1000μm or more x 1000μm or more

[0082] (Chemical Composition)

[0083] The chemical composition of the electromagnetic steel sheet included in the laminated core of the present embodiment is not limited and may be within a known range. However, in order to obtain the above-mentioned {411} <011> In order to obtain excellent magnetic properties with high efficiency, it is preferable to set the chemical composition as shown below.

[0084] In the following description, "%" as a unit of the content of each element means "mass %" unless otherwise specified. In addition, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the upper limit and the lower limit.

[0085] The electromagnetic steel sheet of the laminated core of the present embodiment has a chemical composition that can produce a ferrite-austenite transformation (hereinafter, α-γ transformation) to a certain extent (even if the entire structure is not transformed into γ, a certain amount of γ is produced when heated), and preferably has the following chemical composition: C: 0.0100% or less, Si: 1.50% to 4.00%, sol.Al: 0.0001% to 1.0000%, S: 0.0100% or less, N: 0.0100% or less, Mn, N i, Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn and Cd: 0.0000% to 0.0100% in total, and the remainder is Fe and impurities. Furthermore, the contents of Mn, Ni, Cu, Si, sol.Al and P preferably satisfy the prescribed conditions described below. As impurities, substances contained in raw materials such as ores or wastes, and substances contained in the manufacturing process can be exemplified.

[0086] (C: 0.0100% or less)

[0087] C is an element that precipitates fine carbides and hinders grain growth, thereby increasing iron loss or causing magnetic aging. Therefore, the lower the C content, the better. This phenomenon is significant when the C content exceeds 0.0100%. Therefore, the C content is preferably 0.0100% or less. The C content is more preferably 0.0050% or less, and further preferably 0.0025% or less. The lower limit of the C content is not particularly limited, but based on the cost of decarburization treatment during refining, the C content is preferably 0.0005% or more.

[0088] (Si: 1.50% to 4.00%)

[0089] Si is an element that increases resistance and reduces eddy current loss, reduces iron loss, or increases yield ratio and improves punching workability into the core. When the Si content is less than 1.50%, these effects cannot be fully obtained. Therefore, in order to obtain the above effects, the Si content is preferably 1.50% or more.

[0090] On the other hand, when the Si content exceeds 4.00%, the magnetic flux density decreases or the hardness increases excessively, so that the punching workability decreases or the cold rolling becomes difficult. Therefore, the Si content is preferably 4.00% or less.

[0091] (sol.Al: 0.0001%~1.0000%)

[0092] Sol.Al is an element that increases resistance and reduces eddy current loss, and reduces iron loss. Sol.Al is also an element that helps to increase the relative size of magnetic flux density B50 to saturation magnetic flux density. Here, magnetic flux density B50 refers to the magnetic flux density under a magnetic field of 5000A / m. When the sol.Al content is less than 0.0001%, these effects cannot be fully obtained. In addition, Al also has a desulfurization promoting effect in steelmaking. Therefore, the sol.Al content is preferably 0.0001% or more. The sol.Al content is more preferably 0.0010% or more, and further preferably 0.1000% or more.

[0093] On the other hand, when the sol.Al content exceeds 1.0000%, the magnetic flux density decreases. Therefore, the sol.Al content is preferably 1.0000% or less.

[0094] (S: 0.0100% or less)

[0095] S is not an essential element, but is contained in steel as an impurity. S precipitates as fine MnS, which hinders recrystallization and grain growth during annealing. Therefore, the lower the S content, the better. Such an increase in iron loss and a decrease in magnetic flux density caused by the hindrance of recrystallization and grain growth are significant when the S content exceeds 0.0100%. Therefore, the S content is preferably less than 0.0100%. The lower limit of the S content is not particularly limited, but based on the cost of desulfurization treatment during refining, the S content is preferably greater than 0.0003%.

[0096] (N: 0.0100% or less)

[0097] N is an element that deteriorates magnetic properties by forming fine precipitates such as TiN or AlN. Therefore, the lower the N content, the better. Since such deterioration of magnetic properties is significant when the N content exceeds 0.0100%, the N content is preferably 0.0100% or less. The lower limit of the N content is not particularly limited, but based on the cost of denitrification treatment during refining, the N content is preferably 0.0010% or more.

[0098] (One or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total)

[0099] These elements are necessary for causing the α-γ phase transition, and at least one of these elements is preferably contained in a total amount of 2.50% or more.

[0100] On the other hand, if the total content of these elements exceeds 5.00%, not only the cost increases, but also the magnetic flux density may decrease. Therefore, it is preferable that at least one of these elements is 5.00% or less in total.

[0101] The content of each of Mn, Ni, and Cu is not limited, but from the viewpoint of resistivity, the Mn content is preferably 1.50% or more.

[0102] In addition, as a condition for generating an α-γ phase transition and obtaining good magnetic properties, the following condition is further satisfied. That is, when the Mn content (mass %) is recorded as [Mn], the Ni content (mass %) is recorded as [Ni], the Cu content (mass %) is recorded as [Cu], the Si content (mass %) is recorded as [Si], the sol.Al content (mass %) is recorded as [sol.Al], and the P content (mass %) is recorded as [P], it is preferred to satisfy the following formula (1):

[0103] (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol.Al]+4×[P])≧1.50%…(1).

[0104] When the above-mentioned formula (1) is not satisfied, the α-γ phase transition does not occur, or even if it occurs, the phase transition point is high, so even if the manufacturing method described later is applied, a sufficient magnetic flux density may not be obtained.

[0105] The chemical composition of the electromagnetic steel sheet is basically composed of the above elements, and the balance is Fe and impurities (impurities other than the above), but it can also replace part of the balance of Fe and contain one or more of Co, Sn, Sb, P, Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn and Cd within the range shown below. Since these elements may not necessarily be contained, the lower limit is 0%. In addition, even if these elements are not intentionally added but contained as impurities, it is allowed.

[0106] (Co: 0.000%~1.000%)

[0107] Co is an element that increases magnetic flux density and may therefore be contained as necessary.

[0108] On the other hand, if Co is contained excessively, the cost increases. Therefore, the Co content is preferably 1.000% or less.

[0109] (Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%)

[0110] Sn and Sb are elements that improve the texture after cold rolling and recrystallization and increase the magnetic flux density. Therefore, these elements may be contained as needed. In the case of imparting further effects such as magnetic properties, it is preferred to contain one or more selected from the group consisting of 0.020% to 0.400% Sn and 0.020% to 0.400% Sb.

[0111] On the other hand, if these elements are contained excessively, the steel becomes brittle. Therefore, the Sn content and the Sb content are both 0.400% or less.

[0112] (P: 0.000%~0.400%)

[0113] P is an element effective in ensuring the hardness of the steel sheet after recrystallization. In addition, P is also an element that has a favorable effect on magnetic properties. Therefore, it can also be contained. In the case of achieving these effects, it is preferred that the P content be set to 0.020% or more.

[0114] On the other hand, if P is excessively contained, the steel becomes brittle. Therefore, the P content is preferably 0.400% or less.

[0115] (One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn and Cd: 0.0000% to 0.0100% in total)

[0116] Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn and Cd are elements that react with S in molten steel during casting to form sulfide or oxysulfide or both precipitates. Hereinafter, Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn and Cd are sometimes collectively referred to as "coarse precipitate forming elements". The particle size of the precipitates of the coarse precipitate forming elements is about 1μm to 2μm, which is much larger than the particle size of fine precipitates such as MnS, TiN, AlN (about 100nm). Therefore, these fine precipitates adhere to the precipitates of the coarse precipitate forming elements, making it difficult to hinder the recrystallization and grain growth during annealing such as intermediate annealing. In order to fully achieve these effects, the total amount of these elements is preferably 0.0005% or more. More preferably, it is 0.0010% or more.

[0117] On the other hand, if the total content of these elements exceeds 0.0100%, sulfides or oxysulfides or the total content of both will be excessive, which will inhibit recrystallization and grain growth during annealing such as intermediate annealing. Therefore, the content of coarse precipitate-forming elements is preferably 0.0100% or less in total.

[0118] The chemical composition can be measured by a general analytical method for steel. For example, the chemical composition can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Specifically, the chemical composition is determined by measuring a test piece collected from a steel plate using a specified measuring device under conditions based on a pre-made calibration curve. C and S can be measured using the combustion-infrared absorption method, and N can be measured using the inert gas melting-thermal conductivity method.

[0119] When there is an insulating film on the surface of the electromagnetic steel sheet, it may be subjected to analysis after being mechanically removed by grinding or cutting.

[0120] The laminated core of the present embodiment can achieve its effects as long as it has the above-mentioned features regardless of the manufacturing method. However, it is preferred that the laminated core be manufactured stably according to the following method.

[0121] (I) an insulating film forming step of forming an insulating film having adhesiveness on the surface of the electromagnetic steel sheet,

[0122] (II) A lamination step of punching out the electromagnetic steel sheets on which the insulating coating is formed into a predetermined shape as required, laminating a plurality of the sheets and heat-compression-bonding them to produce a laminated iron core.

[0123] Preferred conditions are described below, but known conditions can be applied to conditions not described.

[0124] <Insulating film forming step>

[0125] In the insulating film forming step, an insulating film having adhesiveness is formed on the electromagnetic steel sheet formed of the base steel sheet. The insulating film may be formed on only one surface or on both surfaces.

[0126] The insulating film is formed by applying a treatment liquid to the base steel plate and then sintering. During sintering, the solidification temperature of the insulating film is set to Tr (°C) in units of °C, and the material is heated in such a manner that the material reaches a temperature Tmax (°C) of less than 200°C and satisfies the following formula (4). In addition, it is preferred that the heating rate is set to 6.0°C / second or less, and the time tr for the material temperature to be above Tr is set to 30 to 60 seconds.

[0127] Tr+30≦Tmax≦Tr+50(4)

[0128] If the ultimate temperature Tmax (° C.) of the material during sintering is 200° C. or higher, there is a concern that the resin may be oxidized.

[0129] When Tmax exceeds Tr+50°C, stress increases due to excessive curing, thereby deteriorating magnetic properties, and when Tmax is less than Tr+30°C, adhesive strength decreases due to insufficient curing.

[0130] In addition, if the heating rate exceeds 6.0°C / second, curing cannot be properly performed and the bonding strength is insufficient. Generally speaking, if the heating rate is slowed down, the furnace length needs to be extended or the production line speed needs to be reduced, which is not preferred in terms of equipment limitations or productivity. However, in the manufacturing method of the laminated core of the present embodiment, based on the new insight that the above-mentioned effect can be obtained by slowing down the heating rate, the heating rate is slowed down instead.

[0131] Here, the curing temperature Tr is the temperature at which the logarithmic decrement rate measured by a rigid pendulum-type physical property tester decreases with curing. If a cross-linked structure appears as the curing reaction proceeds, the movement of the pendulum is restricted and the swing period of the pendulum is sharply reduced. Therefore, the curing temperature Tr can be determined based on the change in the swing period of the pendulum.

[0132] The logarithmic decay rate is measured in accordance with ISO12013-2 using a rigid pendulum test with a rigid pendulum at the edge of a cylinder at a heating rate of 10°C / second. By measuring the logarithmic decay rate, the dynamic viscoelasticity of the coating can be evaluated. The logarithmic decay rate can be measured, for example, using an A&D RPT-3000W or an equivalent rigid pendulum-type physical property testing machine. The measurement temperature range of the logarithmic decay rate can be appropriately set, for example, it can be set from room temperature (25°C) to 300°C.

[0133] Regarding the treatment liquid used to form an insulating coating with bonding ability, it is preferred that an acrylic resin has a certain degree of rigidity after curing to ensure bonding strength and has less compressive stress on the steel plate caused by curing, and the solid content is converted to more than 90% by weight of the entire treatment liquid. As other components, resins or inorganic salts and inorganic particles may also be contained. Resins include epoxy resins, polyurethane resins, phenolic resins, etc. Inorganic salts include phosphates, chromates, borates, etc. Inorganic particles include silicon dioxide, titanium oxide, magnesium oxide, zirconium hydroxide, etc. However, if the inorganic particles are foaming particles, bubbles are generated in the insulating coating, and the adhesion of the coating is reduced, so foaming inorganic particles are not used.

[0134] In addition, from the viewpoint of adhesive strength, the content of inorganic fine particles is preferably 0.05 mass % or less.

[0135] The acrylic resin contained in the treatment liquid is not particularly limited. As the monomer used for the acrylic resin, for example, unsaturated carboxylic acids such as acrylic acid and methacrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate and the like (meth)acrylate can be exemplified. (Meth)acrylate means acrylate or methacrylate. As the acrylic resin, one kind can be used alone, or two or more kinds can be used in combination.

[0136] <Lamination process>

[0137] In the lamination process, the electromagnetic steel sheets with the insulating coating formed thereon are punched into a predetermined shape determined as needed (a shape determined when applied to a stator core or a rotor core), and then heat-pressed to produce a laminated core.

[0138] At this time, in order to make the hardness of the insulating film after the laminated core to be 200 to 300 MPa, it is preferable to set the pressing force to 10 to 60 kgf / cm 2 , the pressure-bonding temperature Tp (° C.) is set to the condition under which the following formula (2) is satisfied.

[0139] Tr+60≦Tp≦Tr+100(2)

[0140] In addition, in the case where the content of A411-011 is set to 15.0% or more in the laminated electromagnetic steel sheets, a production method having the following steps can be applied.

[0141] Hereinafter, in the present embodiment, the Ar3 temperature, the Ar1 temperature, and the Ac1 temperature (all in degrees Celsius) are temperatures obtained by the following method.

[0142] The Ar3 temperature and the Ar1 temperature are obtained based on the thermal expansion change of the steel material (steel plate) during cooling at an average cooling rate of 1°C / sec, and the Ac1 temperature is obtained based on the thermal expansion change of the steel material (steel plate) during heating at an average heating rate of 1°C / sec.

[0143] <Hot rolling process>

[0144] In the hot rolling process, a steel material satisfying a predetermined chemical composition (preferably the above-mentioned chemical composition) is hot-rolled to produce a hot-rolled steel sheet. The hot rolling process includes a heating process and a rolling process.

[0145] The steel material is, for example, a slab manufactured by conventional continuous casting, and the steel material of the above chemical composition is manufactured by a well-known method. For example, molten steel is manufactured by a converter or an electric furnace. The manufactured molten steel is subjected to secondary refining by a degassing device or the like to obtain molten steel having the above chemical composition (the chemical composition does not substantially change in the subsequent steps). The molten steel is used to cast a slab by a continuous casting method or an ingot casting method. The cast slab may also be subjected to bloom rolling.

[0146] In the heating process, the steel material having the above chemical composition is preferably heated to 1000-1200° C. Specifically, the steel material is placed in a heating furnace or a soaking furnace and heated in the furnace. The holding time at the above heating temperature in the heating furnace or soaking furnace is not particularly limited, and is, for example, 1 to 200 hours.

[0147] In the rolling process, the steel material heated by the heating process is subjected to multiple rolling passes to produce hot-rolled steel plates. Here, "pass" means that the steel plate is pressed down by a rolling stand having a pair of working rolls. For example, hot rolling can be performed by tandem rolling using a tandem rolling mill including a plurality of rolling stands arranged in a row (each rolling stand having a pair of working rolls) to perform multiple rolling passes, or by reverse rolling using a pair of working rolls to perform multiple rolling passes. From the perspective of productivity, it is preferred to use a tandem rolling mill to perform multiple rolling passes.

[0148] The rolling in the rolling process (rough rolling and finishing rolling) is preferably performed at a temperature in the γ range (Ar3 temperature or higher). That is, hot rolling is preferably performed so that the temperature at the final pass of finishing rolling (finishing rolling temperature FT (°C)) is Ar3 temperature or higher.

[0149] The finishing temperature FT means the surface temperature (°C) of the steel plate at the exit side of the rolling stand where the final pass of the rolling is performed during the above-mentioned rolling process in the hot rolling process. The finishing temperature FT can be measured, for example, by a thermometer provided at the exit side of the rolling stand where the final pass of the rolling is performed. The finishing temperature FT means, for example, the average value of the temperature measurement results of the portion excluding one area at the front end and one area at the rear end when the entire length of the steel plate is divided into 10 areas in 10 equal parts along the rolling direction.

[0150] <Cooling process>

[0151] In the cooling process, the steel plate (hot-rolled steel plate) after the hot rolling process (after the finish rolling is completed) is cooled. This cooling causes a phase transformation from austenite to ferrite, thereby obtaining moderately fine grains with high strain. As cooling conditions, it is preferred that cooling be started 0.10 seconds after the final pass of the finish rolling (after more than 0.10 seconds), and cooling be performed in such a manner that the surface temperature of the hot-rolled steel plate becomes 300°C or higher and below the Ar1 temperature after 3 seconds (without immediate quenching). By avoiding immediate quenching in this way, no special quenching equipment is required, which is also a manufacturing (cost) advantage. In addition, the texture of the hot-rolled steel plate becomes a structure in which non-recrystallized austenite undergoes phase transformation when quenching is performed immediately, and is easily concentrated in {100} in the structure after the final annealing performed later. <011> On the other hand, it is speculated that if the structure is not immediately quenched, it will be partially recrystallized austenite and undergo phase transformation, and it is easy to gather in {411} in the structure after the final annealing. <011> orientation. That is, in order to improve {411} <011> It is important to achieve a partially recrystallized austenite phase transformation at a high rate, and it is preferred not to perform immediate quenching.

[0152] In addition, as cooling conditions, it is preferable to set the conditions that the average crystal grain size in the hot-rolled steel sheet before cold rolling is 3 to 10 μm. In the appropriate crystal grain size without excessive miniaturization, when cold rolling is performed later, α fibers are developed after intermediate annealing, and {411} which is usually difficult to develop can be made after subsequent skin pass rolling and final annealing. <011> On the other hand, if the grains are too coarse, it is difficult for α fibers to develop after cold rolling and intermediate annealing, and sometimes the desired {411} <011> Rate.

[0153] In order to make the average grain size of the hot-rolled steel sheet before cold rolling 3 to 10 μm, the temperature can be set to a temperature below the Ar1 temperature within 3 seconds after the final pass of the finish rolling. On the other hand, when the cooling stop temperature is less than 300°C, there is a concern that the average grain size of the hot-rolled steel sheet will be excessively refined. Therefore, it is preferred to set the cooling stop temperature to 300°C or above.

[0154] The hot-rolled steel sheet temperature (particularly the finish rolling temperature) and the surface temperature of the hot-rolled steel sheet 3 seconds after the final pass of the finish rolling were measured by the following method.

[0155] In a hot rolling equipment production line for manufacturing electromagnetic steel plates, a cooling device and a conveying line (such as a conveying roller) are arranged downstream of the hot rolling mill, and a thermometer for measuring the surface temperature of the hot-rolled steel plate is arranged on the exit side of the rolling stand that implements the final pass of the hot rolling mill. When a plurality of thermometers are also arranged along the conveying line on the conveying roller arranged downstream of the rolling stand, the hot rolling temperature and the surface temperature of the hot-rolled steel plate 3 seconds after the final pass of finish rolling can be measured using the thermometer arranged in the hot rolling equipment production line.

[0156] The cooling is performed using a cooling device arranged downstream of the rolling stand for the final pass. A plurality of water cooling devices are generally arranged, and a temperature measuring device is arranged at the inlet side of each water cooling device. The cooling device may be, for example, a well-known water cooling device or a well-known forced air cooling device. Preferably, the cooling device is a water cooling device. The coolant of the water cooling device may be water or a mixed fluid of water and air.

[0157] <Cold rolling process>

[0158] In the cold rolling process, the hot rolled steel sheet is cold rolled to obtain a cold rolled steel sheet. In order to develop the α fibers after cold rolling, it is preferred not to perform hot rolled steel sheet annealing before the cold rolling process. The hot rolled steel sheet annealing mentioned here means, for example, a heat treatment at a heating temperature of less than Ac1 temperature and more than 300°C.

[0159] Cold rolling can be performed by, for example, performing tandem rolling using a tandem mill including a plurality of rolling stands arranged in a row (each rolling stand having a pair of working rolls) to perform multiple passes of rolling. Alternatively, rolling can be performed by reverse rolling using a Sendzimir mill having a pair of working rolls or the like to perform one or more passes of rolling. From the viewpoint of productivity, it is preferred to perform multiple passes of rolling using a tandem mill.

[0160] In cold rolling, cold rolling is performed without annealing during the cold rolling. For example, when reverse rolling is performed and cold rolling is performed in multiple passes, multiple passes of cold rolling are performed without annealing between the passes. If annealing is performed between the passes, it is impossible to develop a desired orientation in the process described later.

[0161] The cold rolling can be performed in one pass using a reversing rolling mill. In addition, when cold rolling is performed using a tandem rolling mill, the cold rolling is continuously performed in a plurality of passes (passes in each rolling stand).

[0162] In the present embodiment, in order to develop α fibers, the reduction ratio RR1 (%) in cold rolling is preferably set to 75 to 95%. The reduction ratio RR1 is more preferably 78 to 92%. Here, the reduction ratio RR1 is defined as follows.

[0163] Reduction ratio RR1 (%) = (1-plate thickness after rolling in the final pass of cold rolling / plate thickness before rolling in the first pass of cold rolling) × 100

[0164] <Intermediate annealing process>

[0165] In the intermediate annealing step, intermediate annealing is performed on the steel sheet after the cold rolling step (cold rolled steel sheet).

[0166] In the present embodiment, annealing is preferably performed by heating (heating) at a heating rate of 300° C. / sec or more to an annealing temperature (intermediate annealing temperature T1 ) (° C.) of 600° C. to Ac1 temperature or less.

[0167] When the heating rate to the annealing temperature is less than 300°C / second, there is a concern that sufficient recovery may not be achieved and the desired texture may not be obtained. The heating rate is preferably 400°C / second or more. A faster heating rate is preferred for the formation of texture, but when a heating rate exceeding 2000°C / second is obtained, special equipment or control is required, which greatly increases the cost. Therefore, the heating rate may be set to 2000°C / second or less. More preferably, it is 1000°C / second or less.

[0168] The heating rate is calculated by dividing the temperature change from room temperature (eg, 25° C.) to the annealing temperature by the time required for the heating.

[0169] In addition, if the annealing temperature of the intermediate annealing exceeds the Ac1 temperature, part of the structure of the steel sheet will transform into austenite. Due to the change in crystal orientation accompanying the phase transformation, the subsequent skin-pass rolling and final annealing will {411} <011> Oriented grains cannot grow sufficiently, and the magnetic flux density may not increase.

[0170] On the other hand, if the intermediate annealing temperature is too low, no recrystallization will occur during the subsequent skin pass rolling and final annealing. <011> Oriented grains may not grow sufficiently, and the magnetic flux density may not be increased. Therefore, the intermediate annealing temperature T1 (° C.) is preferably 600° C. or higher.

[0171] The intermediate annealing temperature T1 (° C.) is the sheet temperature (surface temperature) near the extraction port of the annealing furnace.

[0172] The holding time at the intermediate annealing temperature T1 (° C.) in the intermediate annealing step may be a time known to those skilled in the art. The holding time at the intermediate annealing temperature T1 (° C.) is, for example, 5 to 60 seconds, but is not limited thereto.

[0173] The atmosphere during the intermediate annealing is not particularly limited, and for example, a gas containing 20% ​​by volume of H 2 , the rest is composed of N 2 Atmospheric gas (dry) of the composition The cooling rate of the steel sheet after the intermediate annealing is not particularly limited, and is, for example, 5.0 to 60.0° C. / sec.

[0174] <Skin Pass Rolling Process>

[0175] In the skin pass rolling process, the cold rolled steel sheet after the intermediate annealing process is rolled (cold rolled) in a normal temperature atmosphere. For the skin pass rolling here, for example, a reversing mill represented by the Sendzimir mill or a tandem mill is used.

[0176] In the skin pass rolling process, rolling is performed without annealing during the process. For example, when reverse rolling is performed and skin pass rolling is performed in multiple passes, the process is performed without annealing between the passes. It is also possible to perform skin pass rolling in only one pass using a reversing mill. In addition, when skin pass rolling using a tandem mill is performed, rolling is performed continuously in multiple passes (passes in each rolling stand).

[0177] In this embodiment, after strain is introduced into the steel sheet by hot rolling and cold rolling, the strain introduced into the steel sheet is temporarily reduced by intermediate annealing. Then, skin pass rolling is performed. Thus, the strain excessively introduced by cold rolling is reduced in the intermediate annealing, and the intermediate annealing is performed to suppress the preferential recrystallization of {111} grains in the steel sheet surface, so that {411} <011> Then, an appropriate amount of strain is introduced into each grain in the steel sheet during skin pass rolling, so that the steel sheet is in a state where grain growth due to expansion is likely to occur during the final annealing in the next step.

[0178] The reduction ratio RR2 in skin-pass rolling is preferably 10 to 15%. If the reduction ratio RR2 is less than 10%, the strain is too small, and the final annealing time required for grain growth due to expansion becomes longer. On the other hand, if the reduction ratio RR2 exceeds 15%, the strain is too large, causing normal grain growth instead of expansion, and the final annealing time is longer. <148> 、{111} <112> Growth.

[0179] Here, the reduction ratio RR2 is defined as follows.

[0180] Reduction ratio RR2 (%) = (1-plate thickness after final pass of skin-pass rolling / plate thickness before first pass of skin-pass rolling) × 100

[0181] The number of passes in skin-pass rolling may be only one pass (ie, only one rolling pass) or may be a plurality of rolling passes.

[0182] The effect of skin pass rolling performed in this embodiment is significantly different from that of skin pass rolling performed after final annealing. A predetermined structure can be obtained by sequentially performing hot rolling, cooling, cold rolling, intermediate annealing, skin pass rolling, and final annealing under predetermined conditions.

[0183] <Final annealing process>

[0184] In the final annealing process, the steel sheet after the skin-pass rolling process is annealed at an annealing temperature T2 (°C) of 750°C or higher and below the Ac1 temperature for more than 2 hours. When the final annealing temperature T2 (°C) is set to less than 750°C, there is a concern that grain growth due to expansion may not occur sufficiently. In this case, {411} <011> The degree of orientation concentration is reduced.

[0185] On the other hand, when the final annealing temperature T2 (°C) exceeds the Ac1 temperature, part of the structure of the steel sheet transforms into austenite, and grain growth due to expansion does not occur, and the desired {411} <011> Rate.

[0186] In addition, when the annealing time is less than 2 hours, even if the final annealing temperature T2 (°C) is 750°C or higher and below the Ac1 temperature, the grain growth due to expansion cannot be fully achieved, and there is a concern that {411} <011> The degree of orientation concentration is reduced.

[0187] On the other hand, the annealing time of the final annealing is not particularly limited, but the effect is saturated even if the annealing time exceeds 10 hours, so it may be 10 hours or less.

[0188] The heating rate TR2 to the final annealing temperature T2 in the final annealing step may be any heating rate known to those skilled in the art, and is 40° C. / hour or more and less than 200° C. / hour, but is not limited to this range.

[0189] The temperature increase rate TR2 is obtained by the following method.

[0190] A thermocouple is installed on a steel plate having the above chemical composition and subjected to the above hot rolling and skin pass rolling to prepare a sample steel plate. The sample steel plate with the thermocouple installed is heated, and the time from the start of heating to reaching the final annealing temperature T2 is measured. Based on the measured time, the heating rate TR2 is calculated.

[0191] The atmosphere during the final annealing step is not particularly limited. For example, the atmosphere during the final annealing step is set to contain 20% H by volume. 2 , the rest is composed of N 2 The atmosphere gas (dry), or 100% hydrogen (H 2 ) atmosphere, etc. The cooling rate of the steel sheet after the final annealing is not particularly limited. The cooling rate is, for example, 5 to 20°C / sec.

[0192] In the method for manufacturing an electromagnetic steel sheet, for example, shot peening and / or pickling may be performed after the cooling process and before the cold rolling process in the above-mentioned manufacturing process. In shot peening, the hot-rolled steel sheet is shot peened to destroy and remove the oxide scale formed on the surface of the hot-rolled steel sheet. In pickling, the hot-rolled steel sheet is pickled. The pickling treatment uses, for example, an aqueous solution of hydrochloric acid as a pickling bath. The oxide scale formed on the surface of the steel sheet is removed by pickling. Shot peening may be performed after the cooling process and before the cold rolling process, followed by pickling. In addition, pickling may be performed after the cooling process and before the cold rolling process without shot peening. Shot peening may be performed after the cooling process and before the cold rolling process without pickling. Shot peening and pickling are arbitrary processes. Therefore, both the shot peening process and the pickling process may not be performed.

[0193] <Base layer forming step>

[0194] The method for manufacturing the electromagnetic steel sheet of the present embodiment may also form a coating (underlayer) on the surface of the steel sheet (electromagnetic steel sheet) after the final annealing step by coating. For example, the coating may be formed by coating a general treatment agent such as a chromic acid treatment agent or a phosphate treatment agent and sintering the treatment agent.

[0195] Example

[0196] Molten steel was cast to produce an ingot having the chemical composition shown in Table 1. In Table 1, the left side of formula (1) represents the value of the left side of the above formula (1). In addition, the coarse precipitate forming element such as Mg represents the total of one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd.

[0197] Steel sheet No. e has an α-stable component system that does not undergo α-γ transformation.

[0198] The produced ingot was heated to 1150° C. and held for 1 hour, and then hot-rolled. Finish rolling was performed so that the finish rolling temperature FT became the temperature shown in Table 2.

[0199] After the hot rolling was completed (after the final pass), the time until the start of cooling was set as shown in Table 2, and the steel sheet was cooled so that the temperature of the steel sheet 3 seconds after the start of cooling reached the temperature shown in Table 2, and the cooling was stopped at this temperature.

[0200] The hot-rolled steel sheets thus obtained were not subjected to hot-rolled sheet annealing, but were pickled to remove scale, and were cold-rolled at a reduction ratio RR1 shown in Table 2 to produce steel sheets having a sheet thickness of 0.30 mm.

[0201] Then, in an atmosphere consisting of 20% by volume of hydrogen and 80% by volume of nitrogen, the sample was heated to an intermediate annealing temperature T1 shown in Table 2 at a temperature increase rate shown in Table 2, and intermediate annealing was performed by maintaining the temperature at T1 for 30 seconds.

[0202] The steel sheets after intermediate annealing were subjected to skin pass rolling at a reduction ratio RR2 shown in Table 2.

[0203] Next, the skin pass rolled steel sheet was final annealed in a 100% hydrogen atmosphere at a heating rate of 100°C / hour at a final annealing temperature T2 shown in Table 1. At this time, the holding time at the final annealing temperature T2 was set to 2 hours.

[0204] After the final annealing, sintering was performed under the conditions shown in Table 3 to form an insulating film on the surface of the steel sheet.

[0205] Two steel plates of 30 mm×60 mm were cut out from the electromagnetic steel plate having the insulating coating obtained by the above method, and the steel plates were stacked in the plate thickness direction so as to overlap in an area of ​​10 mm×30 mm.

[0206] Thereafter, thermocompression bonding was performed under the conditions shown in Table 3.

[0207] The thickness, hardness and weight average molecular weight of the insulating coating of the electrical steel sheet after the thermocompression bonding were measured according to the above-mentioned method.

[0208] Furthermore, differently from the above, two steel plates of 30 mm×60 mm were cut out from an electromagnetic steel plate having an insulating film on the surface, and the steel plates were stacked in the plate thickness direction so as to overlap in an area of ​​10 mm×30 mm.

[0209] Thereafter, thermocompression bonding was performed under the conditions shown in Table 3.

[0210] [Adhesion strength]

[0211] The adhesive strength was measured by the following method.

[0212] <Analysis Device>

[0213] Automatic plotter AGS-10kNX

[0214] <Measurement Conditions>

[0215] Tensile form: shear tensile test

[0216] Stretching temperature: 25℃

[0217] Stretching speed: 10mm / min

[0218] The tensile test was performed until fracture with n=5, and the average value of the maximum strength until fracture was taken as the adhesive strength.

[0219] The results are shown in Table 4.

[0220] When the adhesive strength is 10.0 MPa or more, it is judged that the adhesive strength is sufficient.

[0221] Different from the above, three 55 mm×55 mm steel plates were cut from an electromagnetic steel plate having an insulating film on the surface, two of which were coated with adhesive so as to overlap the entire surface, and then the steel plates were overlapped in the plate thickness direction. Thereafter, the steel plates were thermocompressed under the conditions shown in Table 3.

[0222] [Magnetic properties]

[0223] The degradation ratio of the magnetic properties of the obtained electrical steel sheets was measured by the following method.

[0224] First, for another sheet different from the two sheets cut out and superimposed, the iron loss W10 / 400 (W / Kg) in the 0° and 90° directions from the rolling direction was measured according to JIS C2556 (2015), and the average value was taken as the iron loss W1 when there was no bonding.

[0225] Then, for the bonded electromagnetic steel sheets, the iron loss W10 / 400 (W / Kg) in the 0° direction and the 90° direction from the rolling direction was measured in accordance with JIS C2556 (2015), and the average value was taken as the iron loss W2 after bonding.

[0226] From W1 and W2, the iron loss degradation rate Wa (%) is calculated based on the following formula.

[0227] Wa=(W2-W1) / W1×100

[0228] The results are shown in Table 4.

[0229] When Wa is 10.0% or less, it is judged that the deterioration of magnetic properties is suppressed.

[0230] [Table 1]

[0231]

[0232] [Table 2]

[0233]

[0234] [Table 3]

[0235]

[0236] [Table 4]

[0237]

[0238] As can be seen from Tables 1 to 4, in Manufacturing Nos. 1 to 5 which are examples of the present invention, the composition and manufacturing conditions of the electromagnetic steel sheet and the composition and manufacturing conditions of the insulating coating are within the scope of the present invention, the hardness of the insulating coating is within the scope of the present invention, the bonding strength is high, and the deterioration of the magnetic properties is small.

[0239] On the other hand, in Nos. 6 to 16 as comparative examples, the predetermined insulating coating was not provided, and the degradation ratio of the adhesive strength or the magnetic characteristics was lower than the target.

[0240] Industrial Availability

[0241] According to the present invention, a laminated core having high bonding strength and excellent magnetic characteristics can be provided. The core can be used in a rotating electric machine and the like, and has high industrial applicability.

[0242] Description of Reference Numerals

[0243] 1-layer laminated core

[0244] 21 Electromagnetic steel plate (base steel plate)

[0245] 22 Insulation coating< / uvw> < / uvw> < / uvw> < / uvw>

Claims

1. A laminated core comprising: a plurality of electromagnetic steel sheets stacked one on another; and an insulating film provided between the electromagnetic steel sheets adjacent to each other in the stacking direction and bonding the electromagnetic steel sheets to each other; The hardness of the insulating film is 200-300 MPa.

2. The laminated core according to claim 1, The weight average molecular weight of the sol component of the insulating film is 10,000 to 100,000.

3. The laminated core according to claim 1 or 2, In the plurality of electromagnetic steel sheets, when {hkl} is measured by SEM-EBSD on a surface parallel to the rolling surface at a depth of 1 / 2 of the sheet thickness from the surface, <uvw> When the area ratio of oriented grains to the entire field of view is represented by Ahkl-uvw, A411-011 is 15.0% or more.< / uvw> 4. The laminated core according to claim 3, The chemical composition of the electromagnetic steel sheet, in terms of mass %, comprises: C: 0.0100% or less, Si: 1.50% to 4.00%, Sol.Al: 0.0001%~1.0000%, S: 0.0100% or less, N: 0.0100% or less, One or more selected from the group consisting of Mn, Ni, and Cu: 2.50% to 5.00% in total, Co: 0.000% to 1.000%, Sn: 0.000%~0.400%, Sb: 0.000%~0.400%, P: 0.000% to 0.400%, and One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total, When the Mn content in mass % is represented by [Mn], the Ni content is represented by [Ni], the Cu content is represented by [Cu], the Si content is represented by [Si], the sol.Al content is represented by [sol.Al], and the P content is represented by [P], the following formula (1) is satisfied: (2×[Mn]+2.5×[Ni]+[Cu])-([Si]+2×[sol.Al]+4×[P])≧1.50%…(1), and the remainder is composed of Fe and impurities.