Low-temperature controllable nitriding method and system based on ammonia decomposition
By using a ruthenium-containing catalyst with a reaction temperature less than 500℃ in ammonia decomposition gas nitriding technology, the nitrogen potential is accurately controlled, and the problems of low accuracy of nitrogen potential control and poor stability of the nitriding process are solved, achieving more efficient and stable The nitriding effect reduces the testing cost and expands the application scenarios.
Patent Information
- Application Number
- CN202410812777.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-22
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing ammonia decomposition gas nitriding technology, the nitrogen potential control accuracy is low, the nitriding process is poor, the application scenarios are limited, and the testing cost is high.
The ammonia decomposition catalyst containing ruthenium groups with a reaction temperature of less than 500℃ was used to perform the ammonia decomposition reaction. By detecting the ammonia decomposition rate and the mixed gas flow rate, the hydrogen partial pressure and ammonia partial pressure were calculated, the nitrogen potential was determined, and the trend relationship diagram was adjusted. The reaction temperature and gas flow rate form a mixed gas with corresponding nitrogen potential for nitriding.
It improves the accuracy of nitrogen potential control and the stability of the nitriding process, reduces testing costs, expands the application range of nitriding technology, and reduces equipment errors and energy consumption.
Smart Images

Figure CN118910537A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ammonia decomposition gas nitriding, and in particular to a low-temperature controllable nitriding method and system based on ammonia decomposition. Background Art
[0002] In the prior art, active nitrogen atoms in nitrogen are diffused into the surface of iron-based alloy parts to obtain higher surface hardness and improve wear resistance. Common nitriding methods include gas nitriding, ion nitriding, low-temperature nitrocarburizing, ZeroFlow gas nitriding technology, accelerated gas nitriding method, and atmospheric pressure plasma nitriding technology; the mechanical properties of the nitriding area vary depending on the material structure. It is guaranteed by the single-phase structure (γ' phase or ε phase) produced by nitriding. For this reason, the composition and ratio of the nitriding white layer must be selected, which can only be achieved through controllable nitriding; however, most of the existing gas nitriding technologies have poor quality stability of workpiece nitriding due to the low control accuracy of nitrogen potential, which greatly limits the application of nitriding technology on parts with complex shapes and high nitriding quality requirements. At present, a small number of technologies use precise automatic control technology to adjust the process curve of the nitriding furnace according to the required theoretical value of nitrogen potential to automatically control the gas atmosphere composition in the furnace. This method requires advanced computers and intelligent monitoring technology, and the equipment precision and cost are high.
[0003] Chinese patent CN1431490A discloses an automatic ammonia decomposition rate measuring instrument, which automatically measures and records the ammonia decomposition rate by connecting a circuit, combining a float on a container containing an aqueous solution and a device that converts the water level height into an electrical signal, and realizes controllable nitriding by adjusting the ammonia ventilation volume and controlling the ammonia decomposition rate to ensure the nitriding quality. This controllable nitriding method controls the ammonia decomposition rate only by the ammonia ventilation volume, has a low control accuracy of the nitrogen potential, and has many influencing factors in the ammonia decomposition process, so the control process is unstable and the result accuracy is not high. Summary of the invention
[0004] In view of the defects of the nitriding control methods in the prior art, such as low nitrogen potential control accuracy, poor stability of the nitriding process, limited application scenarios, and high testing costs, a low-temperature controllable nitriding method and system based on ammonia decomposition is provided, which can accurately control the nitrogen potential, has a stable control process, a wide range of application scenarios, and controllable testing costs.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a low-temperature controllable nitriding method based on ammonia decomposition, comprising the following steps: step 1: passing the heated ammonia into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to perform an ammonia decomposition reaction, and recording the reaction temperature when the ammonia decomposes; step 2: the ammonia undergoes a decomposition reaction to generate a mixed gas containing hydrogen, nitrogen and ammonia, and the corresponding ammonia decomposition rate and the flow rate of the generated mixed gas are detected; step 3: according to the ammonia decomposition rate recorded in step 2, the hydrogen partial pressure and the ammonia partial pressure are calculated respectively; and then according to the calculated hydrogen partial pressure and ammonia partial pressure, the corresponding nitrogen potential is calculated by the following formula:
[0006]
[0007] Step 4: Repeat steps 1 to 3 to obtain multiple groups of reaction temperatures, ammonia decomposition rates, mixed gas flow rates and nitrogen potentials during ammonia decomposition, and use the reaction temperature during ammonia decomposition as the horizontal coordinate, the ammonia decomposition rate and the nitrogen potential as the vertical coordinates to determine the first trend relationship diagram between the reaction temperature during ammonia decomposition and the ammonia decomposition rate and the nitrogen potential; use the mixed gas flow rate as the horizontal coordinate and the nitrogen potential as the vertical coordinate to determine the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential; Step 5: According to the first trend relationship diagram between the reaction temperature during ammonia decomposition and the ammonia decomposition rate and the nitrogen potential determined in step 4, and the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential, the heated ammonia is again introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction, and at the same time adjust the reaction temperature during ammonia decomposition and the flow rate of the generated mixed gas to obtain a mixed gas with a corresponding nitrogen potential; Step 6: Pass the mixed gas with the corresponding nitrogen potential into the workpiece to form a nitriding layer on the surface of the workpiece.
[0008] Furthermore, the ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500° C. is composed of a nickel metal carrier and ruthenium metal, and the nickel metal carrier is loaded with ruthenium metal.
[0009] Further, in step 3, the hydrogen partial pressure is calculated by the following formula:
[0010]
[0011] The ammonia partial pressure is calculated using the following formula:
[0012]
[0013] Where a is the ammonia decomposition rate and P is the system pressure.
[0014] Furthermore, in step five, the reaction temperature range corresponding to the corresponding nitrogen potential is determined through the first trend relationship diagram in combination with the nitrogen potential range to be achieved, and the mixed gas flow range corresponding to the corresponding nitrogen potential is determined through the second trend relationship diagram in combination with the nitrogen potential range to be achieved; then, based on the determined reaction temperature range and the flow range of the mixed gas after ammonia decomposition, the influence trends of the reaction temperature and the mixed gas flow rate on the nitrogen potential are confirmed respectively; thereafter, the heated ammonia is introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction.
[0015] Furthermore, in combination with the nitrogen potential interval to be achieved, the reaction temperatures corresponding to the nitrogen potentials at the interval endpoints are determined according to the following formula, thereby obtaining the reaction temperature interval corresponding to the corresponding nitrogen potential:
[0016]
[0017] Where T is the reaction temperature, unit is K
[0018] Through the second trend relationship diagram, combined with the nitrogen potential range that needs to be achieved, the mixed gas flow range corresponding to the corresponding nitrogen potential is determined; then, based on the determined reaction temperature range and the flow range of the mixed gas after ammonia decomposition, the influence trend of the reaction temperature and the mixed gas flow rate on the nitrogen potential is confirmed; thereafter, the heated ammonia is introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction.
[0019] Furthermore, in step six, the nitriding layer is diffused while the mixed gas is introduced, and the diffusion treatment includes the following steps: raising the temperature to above 480°C and continuing to introduce a mixed gas containing nitrogen, hydrogen and ammonia into the nitriding layer for 1 to 3 hours, and then reducing the temperature to 180 to 200°C.
[0020] The present application also discloses a low-temperature controllable nitriding system based on ammonia decomposition, comprising an ammonia storage device, a heat exchange device, a nitriding device and an exhaust gas treatment system; the heat exchange device is connected to the ammonia storage device and the nitriding device at the same time, and the heat exchange device is used to heat the ammonia gas discharged from the ammonia storage device into the nitriding device; the nitriding device is connected to the exhaust gas treatment system; the nitriding device comprises an ammonia decomposition area and a nitriding area, the ammonia decomposition area is connected to the heat exchange device, the ammonia decomposition area is directly connected to the nitriding area, and the ammonia decomposition area is filled with a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C; the ammonia decomposition area and the nitriding area are respectively connected to corresponding heating devices, and the temperatures of the ammonia decomposition area and the nitriding area are independently controlled by the heating devices connected to each other.
[0021] Furthermore, the heat exchange device is also connected to the exhaust gas treatment system. The heat exchange device can transfer the heat of the exhaust gas discharged from the nitriding device to the ammonia introduced into the nitriding device from the ammonia storage device, and the gas discharged from the nitriding device after heat exchange is introduced into the exhaust gas treatment system.
[0022] Furthermore, the exhaust gas treatment system includes an ammonia decomposition device, an adsorption device and a hydrogen storage device. The ammonia decomposition device includes an upper layer, a middle layer and a lower layer, and the upper layer, the middle layer and the lower layer are connected in sequence. The middle layer is filled with a ruthenium-based or nickel-based catalyst, and the upper layer and the lower layer are both filled with alumina balls. The upper layer is connected to the nitriding device, the lower layer is connected to the adsorption device, and the adsorption device is connected to the hydrogen storage device.
[0023] Furthermore, the exhaust gas treatment system includes an ammonia decomposition device and a combustion device. The ammonia decomposition device includes an upper layer, a middle layer and a lower layer. The upper layer, the middle layer and the lower layer are connected in sequence. The middle layer is filled with a ruthenium-based or nickel-based catalyst. The upper layer and the lower layer are both filled with alumina balls. The upper layer is connected to the nitriding device, and the lower layer is connected to the combustion device.
[0024] The low-temperature controllable nitriding method based on ammonia decomposition described in the present invention performs an ammonia decomposition reaction in an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C, thereby reducing the fluctuation effect of high temperature on the nitrogen potential test process, making the test parameters of the control process more accurate, and also reducing the energy consumption in the nitriding process; combining formulas to calculate the ammonia pressure, nitrogen pressure and nitrogen potential respectively, compared with equipment measurement, reducing the influence of equipment errors on the test results, reducing the test cost and improving the test accuracy; in the nitriding process, the nitrogen potential is analyzed from multiple dimensions and the respective influence trends are determined, which more accurately simulates the nitriding process in ammonia decomposition, thereby more accurately and stably controlling the nitriding process, making the nitrogen potential of the mixed gas closer to the target value, reducing the use of test equipment in the entire nitriding process, reducing the influence caused by the limitations of the test equipment, reducing the control cost, and improving the wide range of application of controllable nitriding. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 This is a schematic structural diagram of a low-temperature controllable nitriding system based on ammonia decomposition according to the present invention;
[0027] Figure 2This is another structural schematic diagram of a low-temperature controllable nitriding system based on ammonia decomposition according to the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The low-temperature controllable nitriding method based on ammonia decomposition of the present invention comprises the following steps:
[0030] Step 1: Passing the heated ammonia gas into an environment containing a ruthenium-based ammonia decomposition catalyst having a reaction temperature of less than 500° C. to perform an ammonia decomposition reaction, and recording the reaction temperature during the decomposition of the ammonia gas;
[0031] Step 2: Ammonia undergoes a decomposition reaction to generate a mixed gas containing hydrogen, nitrogen and ammonia, and the corresponding ammonia decomposition rate and the flow rate of the generated mixed gas are detected;
[0032] Step 3: According to the ammonia decomposition rate recorded in step 2, calculate the hydrogen partial pressure and ammonia partial pressure respectively; then, according to the calculated hydrogen partial pressure and ammonia partial pressure, calculate the corresponding nitrogen potential by the following formula:
[0033]
[0034] Step 4: Repeat steps 1 to 3 to obtain multiple groups of reaction temperatures, ammonia decomposition rates, mixed gas flow rates and nitrogen potentials during ammonia decomposition, and determine a first trend relationship diagram between the reaction temperature during ammonia decomposition, the ammonia decomposition rate and the nitrogen potential, with the reaction temperature during ammonia decomposition as the horizontal coordinate, and the ammonia decomposition rate and the nitrogen potential as the vertical coordinates; determine a second trend relationship diagram between the mixed gas flow rate and the nitrogen potential, with the mixed gas flow rate as the horizontal coordinate and the nitrogen potential as the vertical coordinate;
[0035] Step 5: According to the first trend relationship diagram between the reaction temperature during ammonia decomposition and the ammonia decomposition rate and the nitrogen potential determined in step 4, and the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential; the heated ammonia is again introduced into an environment containing a ruthenium-based ammonia decomposition catalyst having a reaction temperature of less than 500° C. to carry out an ammonia decomposition reaction, and the reaction temperature during ammonia decomposition and the flow rate of the generated mixed gas are comprehensively adjusted to obtain a mixed gas with a corresponding nitrogen potential;
[0036] Step 6: Pass a mixed gas with corresponding nitrogen potential into the workpiece to form a nitriding layer on the surface of the workpiece.
[0037] In step 1, heated ammonia is introduced into a nitriding device for ammonia decomposition, and the reaction temperature of ammonia decomposition is recorded. The nitriding device comprises an ammonia decomposition region and a nitriding region which are connected in sequence. The ammonia decomposition region and the nitriding region are respectively connected to independent heating devices. The temperatures of the ammonia decomposition region and the nitriding region are independently controlled by the heating devices connected to them, so as to achieve accurate temperature control of ammonia decomposition and nitriding processes, reduce the influence of temperature between different processes, and improve the accuracy of test results. A ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500° C. is arranged in the ammonia decomposition region. The ruthenium-based ammonia decomposition catalyst uses nickel metal, such as nickel oxide, as a carrier. Ruthenium metal is loaded on the nickel metal carrier. Therefore, the ruthenium-based ammonia decomposition catalyst has both ruthenium and nickel metal activities. , and can still have 99.5% ammonia decomposition reaction activity at a maximum space velocity of 5000mL / g·h and a temperature environment of 500°C. By using the above-mentioned ammonia decomposition catalyst containing both ruthenium and nickel, ammonia decomposition can be carried out in a lower temperature environment. Compared with the traditional high-temperature environment, by using the above-mentioned ammonia decomposition catalyst containing ruthenium, the heat loss in the ammonia decomposition process can be effectively reduced, thereby improving the temperature detection accuracy in the ammonia decomposition process, reducing the impact of temperature fluctuations and losses on temperature detection, and also reducing the energy consumption of the entire process; ammonia decomposes to generate hydrogen and nitrogen under the catalytic action of the above-mentioned ammonia decomposition catalyst and the heating action of the independently controlled heating device; during the ammonia decomposition process, the ammonia decomposition rate corresponding to different reaction temperatures is recorded by a temperature measuring device.
[0038] In step 2, ammonia undergoes a decomposition reaction to generate a mixed gas containing hydrogen, nitrogen and ammonia, and the corresponding ammonia decomposition rate and the flow rate of the generated mixed gas are detected; wherein the ammonia decomposition rate is detected and recorded by a chromatograph, and the flow rate of the mixed gas is detected to verify the influence of the mixed gas flow rate on the nitrogen potential, and in the subsequent selective control process of the nitrogen potential, a comprehensive consideration of the influence of the mixed gas flow rate on the nitrogen potential is added, so as to better control the ammonia decomposition process and determine relevant parameters, thereby improving the accuracy of the nitrogen potential calculation.
[0039] In step 3, according to the ammonia decomposition rate recorded in step 2, the hydrogen partial pressure and the ammonia partial pressure are calculated respectively. In order to improve the accuracy of the subsequent nitrogen potential calculation and reduce the influence of equipment error, environmental error, etc. on the nitrogen potential calculation, specifically, the hydrogen partial pressure is calculated by the following formula:
[0040]
[0041] The ammonia partial pressure is calculated using the following formula:
[0042]
[0043] Where a is the ammonia decomposition rate, P is the system pressure; the unit of ammonia decomposition rate is %, and the unit of system pressure is MPa.
[0044] After the hydrogen partial pressure and ammonia partial pressure are calculated by the above formula, the corresponding nitrogen potential R is calculated according to the following calculation formula:
[0045]
[0046] In step 4, steps 1 to 3 are repeated, and the heated ammonia is repeatedly introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500° C. to carry out an ammonia decomposition reaction, and multiple groups of reaction temperatures, corresponding ammonia decomposition rates and mixed gas flow rates during ammonia decomposition are obtained, and the corresponding ammonia partial pressure, hydrogen partial pressure and corresponding nitrogen potential are calculated according to the corresponding ammonia decomposition rates. In order to determine the relationship between different reaction temperatures and mixed gas flow rates and the corresponding nitrogen potential, in order to better verify the influence of the reaction temperature and the mixed gas flow rate on the nitrogen potential, and then more accurately and effectively control the nitrogen potential of the gas, at the same time, the nitrogen potential under different reaction temperatures and gas flow rates is also achieved. Specifically, the first trend relationship diagram between the reaction temperature during ammonia decomposition and the ammonia decomposition rate and the nitrogen potential is determined by taking the collected multiple reaction temperature data during ammonia decomposition as the horizontal coordinate, and the ammonia decomposition rate data and the nitrogen potential data as the vertical coordinate; the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential is determined by taking the collected multiple mixed gas flow rate data as the horizontal coordinate, and the nitrogen potential data as the vertical coordinate; thereby confirming the change of the gas nitrogen potential during the ammonia decomposition process from the two dimensions of reaction temperature and mixed gas flow rate, and confirming the influence trend of the reaction temperature and mixed gas flow rate on the gas nitrogen potential, so as to more accurately verify the influence of different parameters on the nitrogen potential and the accurate control of the nitrogen potential.
[0047] In step 5, according to the first trend relationship diagram between the reaction temperature during ammonia decomposition and the ammonia decomposition rate and the nitrogen potential determined in step 4, and the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential; the heated ammonia is introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction, and the reaction temperature during ammonia decomposition and the flow rate of the generated mixed gas are comprehensively adjusted. Specifically, the reaction temperature range corresponding to the corresponding nitrogen potential is determined through the first trend relationship diagram in combination with the nitrogen potential range to be achieved, and the mixed gas flow rate range corresponding to the corresponding nitrogen potential is determined through the second trend relationship diagram in combination with the nitrogen potential range to be achieved; then, according to the determined reaction temperature range and the flow rate range of the mixed gas after ammonia decomposition, the reaction temperature is confirmed. The influence trend of the temperature and the mixed gas flow rate on the nitrogen potential is obtained, and then the heated ammonia is introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction, while controlling the reaction temperature during the ammonia decomposition reaction, and controlling the flow rate of the mixed gas after the ammonia decomposition, so as to obtain a mixed gas containing hydrogen, nitrogen and ammonia with a corresponding nitrogen potential; by reversely determining the corresponding reaction temperature and mixed gas flow rate from a first trend relationship diagram and a second trend relationship diagram respectively representing the reaction temperature and the mixed gas flow rate in combination with the nitrogen potential range to be achieved, the complexity and inaccuracy of multiple tests to determine appropriate parameters are reduced, the test accuracy is improved while the test efficiency is improved, and the gap between the theoretical nitrogen potential value and the actual test process is reduced.
[0048] Among them, in order to further accurately determine the nitrogen potential of the mixed gas, achieve accurate control of the ammonia decomposition rate and the composition of the mixed gas during the decomposition of ammonia, and reduce the errors caused by other test factors, preferably, the reaction temperature range corresponding to the nitrogen potential can also be obtained by the following method: according to the nitrogen potential calculation formula under the standard free energy variable method, combined with the nitrogen potential range to be achieved, the reaction temperature corresponding to the nitrogen potential at the interval endpoint is determined according to the following formula, and then the reaction temperature range corresponding to the corresponding nitrogen potential is obtained. Specifically, the calculation formulas for the theoretical nitrogen potential are as follows:
[0049]
[0050] Where T is the reaction temperature, unit is K
[0051] In step six, a mixed gas with a corresponding nitrogen potential is introduced into the workpiece to form a nitriding layer on the surface of the workpiece, completing the nitriding process. Preferably, the nitriding layer is diffused during the introduction of the mixed gas, and the diffusion treatment includes the following steps: raising the temperature to above 480°C and continuing to introduce a mixed gas containing nitrogen, hydrogen and ammonia into the nitriding layer for 1 to 3 hours, and then lowering the temperature to 180 to 200°C; this can promote the diffusion of nitrogen atoms from the surface of the workpiece to the inside, forming a nitrided layer, thereby improving the surface performance of the workpiece.
[0052] Example 1
[0053] Step 1: Pass the heated ammonia gas into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to perform an ammonia decomposition reaction. The reaction temperature during the ammonia decomposition is recorded to be 392.8°C.
[0054] Step 2: Ammonia undergoes a decomposition reaction to generate a mixed gas containing hydrogen, nitrogen and ammonia. The corresponding ammonia decomposition rate is 48.36%, and the flow rate of the generated mixed gas is 73 standard cubic meters;
[0055] Step 3: According to the ammonia decomposition rate recorded in step 2, calculate the hydrogen partial pressure and ammonia partial pressure respectively; then, according to the calculated hydrogen partial pressure and ammonia partial pressure, calculate the corresponding nitrogen potential of 2.36 by the formula:
[0056] Step 4: Repeat steps 1 to 3 to obtain multiple groups of reaction temperatures, ammonia decomposition rates, mixed gas flow rates and nitrogen potentials during ammonia decomposition, as follows:
[0057] Reaction temperature (℃) Ammonia decomposition rate (%) Mixed gas flow rate (standard) Nitrogen potential 392.8 48.36 73 2.36 386.8 44.80 77 2.83 376.5 37.30 80 4.23
[0058] Taking the reaction temperature during ammonia decomposition as the horizontal coordinate, and the ammonia decomposition rate and the nitrogen potential as the vertical coordinate, a first trend relationship diagram between the reaction temperature during ammonia decomposition, the ammonia decomposition rate and the nitrogen potential is determined; taking the mixed gas flow rate as the horizontal coordinate, and the nitrogen potential as the vertical coordinate, a second trend relationship diagram between the mixed gas flow rate and the nitrogen potential is determined;
[0059] Step 5: According to the first trend relationship diagram between the reaction temperature during ammonia decomposition determined in step 4 and the ammonia decomposition rate and nitrogen potential, and the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential; the heated ammonia is introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction, and the ammonia decomposition rate and nitrogen potential are adjusted and controlled within the ammonia decomposition reaction temperature range of 376.5 to 392.8°C and the mixed gas flow rate range of 73 to 80 standard cubic meters; that is, when the reaction temperature increases, the mixed gas flow rate is correspondingly reduced to obtain an accurate nitrogen potential.
[0060] Step 6: Pass a mixed gas with corresponding nitrogen potential into the workpiece to form a nitriding layer on the surface of the workpiece. During the process of passing the mixed gas, the temperature is increased to 490°C, and a mixed gas containing nitrogen, hydrogen and ammonia is continued to be passed into the nitriding layer for 1 hour, after which the temperature is reduced to 180°C to form a nitrided layer.
[0061] Example 2
[0062] Step 1: Pass the heated ammonia gas into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to perform an ammonia decomposition reaction. The reaction temperature during the ammonia decomposition is recorded to be 371.6°C.
[0063] Step 2: Ammonia undergoes a decomposition reaction to generate a mixed gas containing hydrogen, nitrogen and ammonia. The corresponding ammonia decomposition rate is 33.58%, and the flow rate of the generated mixed gas is 88 standard cubic meters;
[0064] Step 3: According to the ammonia decomposition rate recorded in step 2, calculate the hydrogen partial pressure and ammonia partial pressure respectively; then, according to the calculated hydrogen partial pressure and ammonia partial pressure, calculate the corresponding nitrogen potential of 5.25 by the formula:
[0065] Step 4: Repeat steps 1 to 3 to obtain multiple groups of reaction temperatures, ammonia decomposition rates, mixed gas flow rates and nitrogen potentials during ammonia decomposition, as follows:
[0066] Reaction temperature (℃) Ammonia decomposition rate (%) Mixed gas flow rate (standard) Nitrogen potential 353.3 22.18 108 11.46 362.7 28.03 95 7.46 371.6 33.58 88 5.25
[0067] Taking the reaction temperature during ammonia decomposition as the horizontal coordinate, and the ammonia decomposition rate and the nitrogen potential as the vertical coordinate, a first trend relationship diagram between the reaction temperature during ammonia decomposition, the ammonia decomposition rate and the nitrogen potential is determined; taking the mixed gas flow rate as the horizontal coordinate, and the nitrogen potential as the vertical coordinate, a second trend relationship diagram between the mixed gas flow rate and the nitrogen potential is determined;
[0068] Step 5: According to the first trend relationship diagram between the reaction temperature during ammonia decomposition and the ammonia decomposition rate and the nitrogen potential determined in step 4, and the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential; adjust and control the ammonia decomposition rate and the nitrogen potential within the ammonia decomposition reaction temperature range of 353.3 to 371.6°C and the mixed gas flow rate range of 88 to 108 standard cubic meters; that is, when the reaction temperature increases, the mixed gas flow rate is correspondingly increased to obtain an accurate nitrogen potential
[0069] Step 6: A mixed gas with corresponding nitrogen potential is passed through the workpiece to form a nitriding layer on the surface of the workpiece. During the process of introducing the mixed gas, the temperature is increased to 500°C, and a mixed gas containing nitrogen, hydrogen and ammonia is continued to be introduced into the nitriding layer for 2 hours, after which the temperature is reduced to 190°C to form a nitrided layer.
[0070] Example 3
[0071] Step 1: Pass the heated ammonia gas into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to perform an ammonia decomposition reaction. The reaction temperature during the ammonia decomposition is recorded as 450.7°C.
[0072] Step 2: Ammonia undergoes a decomposition reaction to generate a mixed gas containing hydrogen, nitrogen and ammonia. The corresponding ammonia decomposition rate is detected to be 90.223%, and the flow rate of the generated mixed gas is 39 standard cubic meters;
[0073] Step 3: According to the ammonia decomposition rate recorded in step 2, calculate the hydrogen partial pressure and ammonia partial pressure respectively; then, according to the calculated hydrogen partial pressure and ammonia partial pressure, calculate the corresponding nitrogen potential as 0.175 by the formula:
[0074] Step 4: Repeat steps 1 to 3 to obtain multiple groups of reaction temperatures, ammonia decomposition rates, mixed gas flow rates and nitrogen potentials during ammonia decomposition, as follows:
[0075] Reaction temperature (℃) Ammonia decomposition rate (%) Mixed gas flow rate (standard) Nitrogen potential 450.7 90.22 39 0.175 461 93.37 35 0.112 490 97.09 32 0.046
[0076] Taking the reaction temperature during ammonia decomposition as the horizontal coordinate, and the ammonia decomposition rate and the nitrogen potential as the vertical coordinate, a first trend relationship diagram between the reaction temperature during ammonia decomposition, the ammonia decomposition rate and the nitrogen potential is determined; taking the mixed gas flow rate as the horizontal coordinate, and the nitrogen potential as the vertical coordinate, a second trend relationship diagram between the mixed gas flow rate and the nitrogen potential is determined;
[0077] Step 5: According to the first trend relationship diagram between the reaction temperature during ammonia decomposition determined in step 4 and the ammonia decomposition rate and nitrogen potential, and the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential; within the ammonia decomposition reaction temperature range of 450.7 to 490°C and the mixed gas flow rate range of 32 to 39 standard cubic meters, adjust and control the ammonia decomposition rate and nitrogen potential; that is, when the reaction temperature increases, the mixed gas flow rate is correspondingly reduced to obtain an accurate nitrogen potential
[0078] Step 6: Pass a mixed gas with corresponding nitrogen potential into the workpiece to form a nitriding layer on the workpiece surface. During the process of passing the mixed gas, the temperature is raised to 520°C, and a mixed gas containing nitrogen, hydrogen and ammonia is continued to be passed into the nitriding layer for 3 hours, after which the temperature is lowered to 200°C to form a nitriding layer.
[0079] like Figure 1 and Figure 2 The present application also discloses a low-temperature controllable nitriding system based on ammonia decomposition, comprising an ammonia storage device 1, a heat exchange device 2, a nitriding device 3 and an exhaust gas treatment system 4;
[0080] The heat exchange device 2 is connected to the ammonia storage device 1 and the nitriding device 3 at the same time, and the heat exchange device 2 is used to heat the ammonia gas discharged from the ammonia storage device 1 into the nitriding device 3; the nitriding device 3 is connected to the tail gas treatment system 4;
[0081] The nitriding device 3 includes an ammonia decomposition area 31 and a nitriding area 32. The ammonia decomposition area 31 is connected to the heat exchange device 2. The ammonia decomposition area 31 is directly connected to the nitriding area 32. The ammonia decomposition area 31 is filled with a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C. The ammonia decomposition area 31 and the nitriding area 32 are respectively connected to corresponding heating devices. The outer wall of the nitriding device 3 is covered with a thermal insulation material 33.
[0082] The nitriding device 3 is a vertical tubular structure arranged in line, the upper part of the nitriding device 3 is an ammonia decomposition area 31, and the lower part of the nitriding device 32 is a nitriding area. The ammonia decomposition area 31 is directly connected to the nitriding area 32 through a pipeline. The ammonia decomposition area 31 is filled with a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C. The upper part is provided with an ammonia inlet 301, and the upper part is connected to the heat exchange device 2 through the ammonia inlet 301. The lower part is provided with a decomposition gas outlet 302, and the decomposition gas outlet 302 is connected to the exhaust gas treatment system 4. 1 is filled with a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C. Compared with the traditional high-temperature ammonia decomposition catalyst, the influence of high temperature on the test results and possible damage can be reduced during the test of nitrogen potential, so that the test results can be more accurate. At the same time, the use of the ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C also reduces the heat loss in the ammonia decomposition process, reduces the energy consumption, and improves the accuracy of the test results, which is beneficial to the process control of the nitriding test; ammonia decomposes under the catalytic action of the ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to generate a mixture containing nitrogen, hydrogen and ammonia. The mixed gas obtained after decomposition directly enters the nitriding area 32 from the ammonia decomposition area 31, and a nitriding layer is formed on the surface of the workpiece in the nitriding area 32, completing the controllable nitriding process; in order to avoid the generation of nitriding defects during the nitriding process, the process of polishing the nitriding layer after heat treatment is omitted and the production cost is reduced. Specifically, the nitriding layer is diffused during the nitriding process, and the diffusion treatment includes the following steps: raising the temperature to above 480°C and continuing to pass the nitriding layer into the generated mixed gas containing nitrogen, hydrogen and ammonia for 1 to 3 hours, and then reducing the temperature to 180 to 200°C; this can promote the nitrogen atoms Diffusion from the surface of the workpiece to the inside forms a nitrided layer, thereby improving the surface properties of the workpiece; at the same time, the ammonia decomposition area 31 and the nitriding area 32 are respectively connected to an independent first heating device and a second heating device, such as an annular ceramic heating plate or a resistance wire, and the temperatures of the ammonia decomposition area 31 and the nitriding area 32 are independently controlled to make the controllable nitriding process more accurate, reduce the mutual influence of heat during ammonia decomposition and nitriding, and improve the accuracy of the detected data; the outside of the nitriding device 3 is covered with a thermal insulation material to reduce heat loss during ammonia decomposition and nitriding, improve the accuracy of the test results and reduce energy consumption.
[0083] In order to increase the energy of the exhaust gas discharged from the nitriding device 3 after nitriding and reduce the energy consumption of the entire system, preferably, the heat exchange device 2 is also connected to the exhaust gas treatment system 4 and the nitriding device 3 at the same time, and the heat exchange device 2 can transfer the heat of the exhaust gas discharged from the nitriding device 3 to the ammonia introduced into the nitriding device 3 from the ammonia storage device 1, so as to heat the ammonia, thereby reducing the additional heat required for heating the ammonia, and the gas discharged from the nitriding device 3 after heat exchange is continuously introduced into the exhaust gas treatment system for exhaust gas treatment.
[0084] The tail gas after the controllable nitriding process is discharged from the decomposition gas outlet 302 of the nitriding device 3 and enters the tail gas treatment system 4 for tail gas treatment. The tail gas treatment system 4 includes an ammonia decomposition device 41, an adsorption device 42 or a combustion device 44. The ammonia decomposition device 41 includes an upper layer 411, a middle layer 412 and a lower layer 413. The upper layer 411, the middle layer 412 and the lower layer 413 are connected in sequence. The middle layer 412 is filled with a ruthenium-based or nickel-based catalyst. The upper layer 411 and the lower layer 413 are both filled with alumina balls, wherein the microporous surface of the alumina balls has good wear resistance and high temperature resistance required for catalysis, and can prevent the catalyst from being damaged. The upper layer 411 is connected to the nitriding device 3, and the tail gas discharged from the nitriding device 3 enters The ammonia decomposition device 41 is introduced into the ammonia decomposition device 41 and is discharged after passing through the upper layer 411, the middle layer 412 and the lower layer 413 in sequence, so as to further decompose the residual ammonia in the gas into hydrogen and nitrogen, thereby reducing the harm caused by the discharge of ammonia into the air; the decomposed gas is discharged from the lower layer 413 and introduced into the adsorption device 42 or the combustion device 44, wherein the adsorption device 42 is used to further adsorb the ammonia in the decomposed gas, and the adsorption device 42 is connected to the hydrogen storage device 43, and the decomposed gas after adsorption is introduced from the adsorption device into the hydrogen storage device 43 for hydrogen storage and subsequent application; the combustion device 44 is used to further burn the gas discharged from the lower layer 413 and then empty it, thereby reducing the safety hazard caused by the discharge of hydrogen into the air.
[0085] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. However, the obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A low-temperature controllable nitriding method based on ammonia decomposition, characterized in that: The steps include: Step 1: Passing the heated ammonia gas into an environment containing a ruthenium-based ammonia decomposition catalyst having a reaction temperature of less than 500° C. to perform an ammonia decomposition reaction, and recording the reaction temperature during the decomposition of the ammonia gas; Step 2: Ammonia undergoes a decomposition reaction to generate a mixed gas containing hydrogen, nitrogen and ammonia, and the corresponding ammonia decomposition rate and the flow rate of the generated mixed gas are detected; Step 3: According to the ammonia decomposition rate recorded in step 2, calculate the hydrogen partial pressure and ammonia partial pressure respectively; then, according to the calculated hydrogen partial pressure and ammonia partial pressure, calculate the corresponding nitrogen potential by the following formula: Step 4: Repeat steps 1 to 3 to obtain multiple groups of reaction temperatures, ammonia decomposition rates, mixed gas flow rates and nitrogen potentials during ammonia decomposition, and determine a first trend relationship diagram between the reaction temperature during ammonia decomposition, the ammonia decomposition rate and the nitrogen potential, with the reaction temperature during ammonia decomposition as the horizontal coordinate, and the ammonia decomposition rate and the nitrogen potential as the vertical coordinates; determine a second trend relationship diagram between the mixed gas flow rate and the nitrogen potential, with the mixed gas flow rate as the horizontal coordinate and the nitrogen potential as the vertical coordinate; Step 5: According to the first trend relationship diagram between the reaction temperature during ammonia decomposition and the ammonia decomposition rate and the nitrogen potential determined in step 4, and the second trend relationship diagram between the mixed gas flow rate and the nitrogen potential, the heated ammonia is again introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500° C. to carry out an ammonia decomposition reaction, and at the same time, the reaction temperature during ammonia decomposition and the flow rate of the generated mixed gas are adjusted to obtain a mixed gas with a corresponding nitrogen potential; Step 6: Pass a mixed gas with corresponding nitrogen potential into the workpiece to form a nitriding layer on the surface of the workpiece.
2. A low-temperature controllable nitriding method based on ammonia decomposition according to claim 1, characterized in that: The ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500° C. is composed of a nickel metal carrier and ruthenium metal, wherein the nickel metal carrier is loaded with ruthenium metal.
3. A low-temperature controllable nitriding method based on ammonia decomposition according to claim 1, characterized in that: In step 3, the hydrogen partial pressure is calculated using the following formula: The ammonia partial pressure is calculated using the following formula: Where a is the ammonia decomposition rate and P is the system pressure.
4. A low-temperature controllable nitriding method based on ammonia decomposition according to claim 1, characterized in that: In step five, the reaction temperature range corresponding to the corresponding nitrogen potential is determined through the first trend relationship diagram in combination with the nitrogen potential range to be achieved, and the mixed gas flow range corresponding to the corresponding nitrogen potential is determined through the second trend relationship diagram in combination with the nitrogen potential range to be achieved; then, based on the determined reaction temperature range and the flow range of the mixed gas after ammonia decomposition, the influence trends of the reaction temperature and the mixed gas flow rate on the nitrogen potential are confirmed respectively; thereafter, the heated ammonia is introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction.
5. A low-temperature controllable nitriding method based on ammonia decomposition according to claim 1, characterized in that: In step 5, based on the nitrogen potential interval to be achieved, the reaction temperatures corresponding to the nitrogen potentials at the interval endpoints are determined according to the following formula, thereby obtaining the reaction temperature interval corresponding to the corresponding nitrogen potential: Where T is the reaction temperature, unit is K Through the second trend relationship diagram, combined with the nitrogen potential range that needs to be achieved, the mixed gas flow range corresponding to the corresponding nitrogen potential is determined; then, based on the determined reaction temperature range and the flow range of the mixed gas after ammonia decomposition, the influence trend of the reaction temperature and the mixed gas flow rate on the nitrogen potential is confirmed; thereafter, the heated ammonia is introduced into an environment containing a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C to carry out an ammonia decomposition reaction.
6. A low-temperature controllable nitriding method based on ammonia decomposition according to claim 1, characterized in that: In step six, the nitriding layer is diffused during the introduction of the mixed gas, and the diffusion treatment includes the following steps: raising the temperature to above 480°C and continuing to introduce a mixed gas containing nitrogen, hydrogen and ammonia into the nitriding layer for 1 to 3 hours, and then reducing the temperature to 180 to 200°C.
7. A low-temperature controllable nitriding system based on ammonia decomposition, comprising an ammonia storage device, a heat exchange device, a nitriding device and an exhaust gas treatment system; characterized in that: The heat exchange device is connected to the ammonia storage device and the nitriding device at the same time, and the heat exchange device is used to heat the ammonia gas discharged from the ammonia storage device into the nitriding device; the nitriding device is connected to the tail gas treatment system; The nitriding device comprises an ammonia decomposition area and a nitriding area, the ammonia decomposition area is connected to the heat exchange device, the ammonia decomposition area is directly connected to the nitriding area, and the ammonia decomposition area is filled with a ruthenium-based ammonia decomposition catalyst with a reaction temperature of less than 500°C; The ammonia decomposition region and the nitriding region are respectively connected to corresponding heating devices, and the temperatures of the ammonia decomposition region and the nitriding region are independently controlled by the respectively connected heating devices.
8. A low temperature controllable nitriding system based on ammonia decomposition according to claim 7, characterized in that: The heat exchange device is also connected to the exhaust gas treatment system. The heat exchange device can transfer the heat of the exhaust gas discharged from the nitriding device to the ammonia introduced into the nitriding device from the ammonia storage device, and the gas discharged from the nitriding device after heat exchange is introduced into the exhaust gas treatment system.
9. A low-temperature controllable nitriding system based on ammonia decomposition according to claim 7, characterized in that: The exhaust gas treatment system includes an ammonia decomposition device, an adsorption device and a hydrogen storage device. The ammonia decomposition device includes an upper layer, a middle layer and a lower layer. The upper layer, the middle layer and the lower layer are connected in sequence. The middle layer is filled with a ruthenium-based or nickel-based catalyst. The upper layer and the lower layer are both filled with alumina balls. The upper layer is connected to the nitriding device, the lower layer is connected to the adsorption device, and the adsorption device is connected to the hydrogen storage device.
10. A low temperature controllable nitriding system based on ammonia decomposition according to claim 7, characterized in that: The exhaust gas treatment system includes an ammonia decomposition device and a combustion device. The ammonia decomposition device includes an upper layer, a middle layer and a lower layer. The upper layer, the middle layer and the lower layer are connected in sequence. The middle layer is filled with a ruthenium-based or nickel-based catalyst. The upper layer and the lower layer are both filled with alumina balls. The upper layer is connected to the nitriding device, and the lower layer is connected to the combustion device.