Synthesis and preparation method of PEDOT polymer

By using camphorsulfonic acid as a dopant and electrochemical polymerization, the production process of PEDOT polymer is simplified, the problems of complex production and poor solubility in the prior art are solved, and high-efficiency and low-cost PEDOT polymer synthesis is achieved. Suitable for industrial production.

CN118910626AActive Publication Date: 2024-11-08ZHANHUA DARONG CHEM TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410982713.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The production process of existing PEDOT polymers is complex, has a long production time, many by-products, and has poor solubility, making it difficult to produce industrially.

Method used

Camphorsulfonic acid is used as a dopant, and electrochemical polymerization is carried out through electrochemical polymerization using appropriate electrodes to simplify the process flow, improve conductivity and solubility, and shorten the reaction time.

Benefits of technology

It realizes the synthesis of PEDOT polymers with simple process and high yield, shortens production time and reduces costs, and the by-product is a harmless gas, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910626A_ABST
    Figure CN118910626A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and provides a synthesis method of a PEDOT polymer. According to the synthesis method of the PEDOT polymer, EDOT (3, 4-ethylenedioxythiophene) is used as a starting raw material, conductive glass, glassy carbon, a platinum sheet, foamed nickel and foamed cobalt are used as working electrodes or counter electrodes, dimethyl carbonate is used as an electrolyte solution, electrochemical polymerization is carried out under the stirring condition, and the PEDOT polymer is obtained. The PEDOT polymer with high conductivity and high solubility is obtained. The method is easy and convenient to operate, high in yield and capable of being industrially applied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a method for synthesizing and preparing a PEDOT polymer. Background Art

[0002] Poly (3,4-ethylenedioxythiophene) (hereinafter referred to as PEDOT) is a conductive polymer formed by chemical polymerization or electrochemical polymerization of 3,4-ethylenedioxythiophene (EDOT). Since pure PEDOT has poor solubility and the industrial production effect is not as expected, organic or inorganic acids are often used as dopants in the market to improve this drawback. The chemical structure of PEDOT makes it have the characteristics of small energy gap, high conductivity, good environmental stability, high mechanical strength and high visible light transmittance in the doped state. It is widely used in organic thin-film solar cell materials, OLED materials, electrochromic materials, transparent electrode materials and other fields, especially suitable for modifying synthetic electrode materials.

[0003] In recent years, reports have shown that polystyrene sulfonic acid-doped PEDOT produces poly(3,4-ethylenedioxythiophene):polystyrene sulfonic acid polymers, namely PEDOT:PSS polymers. These polymers not only possess most of the advantages of pure PEDOT, but also greatly improve its solubility in aqueous solutions and organic solvents. The only drawback is that the production process of PEDOT:PSS polymers is complicated, the production time is long, and there are many by-products. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a method for synthesizing and preparing a PEDOT polymer. The preparation method uses camphorsulfonic acid as a dopant, which can not only improve the conductivity by increasing the density of charge carriers, but also improve the solubility of the polymer by weakening the interaction between polymer chains. The method for synthesizing and preparing a PEDOT polymer provided by the present invention has a simple process, high yield, and can be industrialized.

[0005] The reaction principle is:

[0006]

[0007] The synthetic preparation method of the present invention comprises the following steps:

[0008] (1) Preparation of electrolyte solution: Dissolve a certain amount of dopant in carbonate solution, heat and stir at 40°C until the dopant is dissolved, and then add EDOT and catalyst.

[0009] (2) Using any one of platinum sheet, glassy carbon, nickel foam, cobalt foam, and conductive glass ITO as a counter electrode and any one of platinum sheet, glassy carbon, nickel foam, and cobalt foam as a working electrode, immersing the pretreated electrode in a prepared electrolyte solution, and performing an electrochemical polymerization reaction under stirring conditions to obtain a product.

[0010] Preferably, the carbonate solution in (1) is dimethyl carbonate;

[0011] Preferably, the catalyst in (1) is hexamethylphosphoric triamide;

[0012] Preferably, the doping agent in (1) is camphorsulfonic acid;

[0013] Preferably, the concentration of EDOT in (1) is 0.1-0.2 mol / L, the concentration of hexamethylphosphoric acid triamide is 0.01-0.5 mol / L, and the concentration of camphorsulfonic acid is 0.1-0.2 mol / L;

[0014] Preferably, the electrochemical polymerization current density in (2) is 5-15 mA / cm 2 ;

[0015] Preferably, the electrochemical polymerization time in (2) is 2-4 h;

[0016] Preferably, in (2), whether the platinum sheet is used as a counter electrode or a working electrode, the pretreatment method thereof is: ultrasonically cleaned in a 1 mol / L hydrochloric acid solution for 5 min, then repeatedly rinsed with deionized water and ethanol, and dried;

[0017] Preferably, (2) glassy carbon is used as the working electrode, and its pretreatment method is: polishing with 0.05 μm Al2O3 powder, rinsing with deionized water and anhydrous ethanol, and drying;

[0018] Preferably, the nickel foam or cobalt foam in (2), whether used as a counter electrode or a working electrode, is pretreated by ultrasonic cleaning in an acetone solution for 10 min, rinsing with deionized water, ultrasonic cleaning in a 1 mol / L hydrochloric acid solution for 10 min, and finally repeatedly rinsing with deionized water and ethanol, and drying;

[0019] Preferably, the pretreatment method of the glassy carbon or conductive glass ITO used as the counter electrode in (2) is: immersing the electrode in a sodium hydroxide solution (0.1 mol / L) for about 20 min, repeatedly washing with deionized water until neutral, rinsing with anhydrous ethanol after washing, and drying;

[0020] Preferably, the contact area between the counter electrode and the working electrode used in (2) and the electrolyte solution is 10 mm×20 mm (the volume of the electrolyte solution is 80 mL).

[0021] The present invention relates to a method for synthesizing a PEDOT polymer, which uses 3,4-ethylenedioxythiophene as a raw material and selects a suitable electrode for electrochemical polymerization of poly 3,4-ethylenedioxythiophene. Compared with other existing methods, it has the following characteristics:

[0022] (1) Rapid reaction, only 2-4 hours is required, which greatly shortens the polymerization reaction time and improves production efficiency;

[0023] (2) The production process is simple to operate. It only requires the preparation of electrolyte solution and pretreatment of the working electrode and the counter electrode before the electrochemical polymerization reaction can be carried out, and the yield can reach 78.9%;

[0024] (3) Low cost, easy industrial production, and easy waste treatment. For example, the byproducts of the electrochemical polymerization reaction in Example 1 are only oxygen and hydrogen, which have no side effects on humans. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the cyclic voltammetry test diagram in Example 1;

[0026] Figure 2 This is the molecular weight distribution diagram in Example 1. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in conjunction with specific implementation methods.

[0028] Example 1

[0029] (1) Preparation of electrolyte solution:

[0030] Weigh 1.74 g of camphorsulfonic acid and dissolve it in 75 mL of dimethyl carbonate solution, stir at 40° C. until the camphorsulfonic acid is completely dissolved, and then add 1.07 g of EDOT and 0.134 g of hexamethylphosphoric acid triamide to obtain an electrolyte solution with a volume of 80 mL;

[0031] (2) Electrode pretreatment:

[0032] The platinum sheet was used as the counter electrode and the glassy carbon electrode was used as the working electrode. The two electrodes were pretreated accordingly. Platinum sheet electrode pretreatment: ultrasonically cleaned in 1 mol / L hydrochloric acid solution for 5 minutes, then rinsed repeatedly with deionized water and ethanol, and dried. Glassy carbon electrode pretreatment: polished with 0.05 μm Al2O3 powder, rinsed with deionized water and anhydrous ethanol, and dried.

[0033] (3) Electrochemical polymerization reaction and electrochemical testing:

[0034] Using an electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd., DZ202201), the pretreated platinum electrode and glassy carbon electrode in (2) were placed in the electrolyte solution in (1). The contact area between the two electrodes and the electrolyte solution was 10 mm × 20 mm. Then, electrochemical polymerization was carried out under stirring conditions. The current density was set to 15 mA / cm 2 , the reaction time was 2h, and PEDOT polymer was obtained.

[0035] During the polymerization process, bubbles were observed to be generated at the platinum electrode, bubbles were generated at the glassy carbon electrode, uniform blue-black substances were generated, and there were black products in the solution. Cyclic voltammetry tests were performed on the polymerization process.

[0036] Cyclic voltammetry test: Scan at a scan rate of 50mV / s (activate first, and then start the test after stabilization). Figure 1 , oxidation peak and reduction peak current can be observed, indicating that an oxidation reaction occurs on the working electrode, i.e., the glassy carbon electrode, and the bubbles generated are oxygen. Correspondingly, a reduction reaction occurs on the counter electrode, i.e., the platinum electrode, and electrons are gained to generate hydrogen. In addition, EDOT is polymerized on the platinum electrode, and the polymerization product is a blue-black substance.

[0037] The blue-black substance on the platinum electrode and the black product in the electrolyte solution were washed with ethanol and dried at 55° C. for 12 h to obtain the final product. The weight of the final product was 0.844 g, and the yield was 78.9%.

[0038] Yield calculation formula:

[0039]

[0040] (4) Characterization of final product:

[0041] At 25°C, No. 7021 was used as a blank control, no product was taken, and only N,N-dimethylformamide (DMF) was tested using a NDJ-8S digital viscometer;

[0042] Samples numbered 7022, 7023, 7024, and 7025 from the same batch of products were taken. The above numbers refer to 0.05 g, 0.1 g, 0.2 g, and 0.3 g of the final product obtained in (3), respectively. The samples were dissolved in 80 mL of N,N-dimethylformamide (DMF) and tested using a NDJ-8S digital viscometer. The data are shown in Table 1.

[0043] Table 1 Viscosity data of different final product qualities

[0044]

[0045]

[0046] In this digital viscometer, to ensure accuracy, the range percentage reading should be controlled between 10%-90% during measurement, and close to 50% is optimal.

[0047] As shown in Table 1, the viscosity of No. 7024 is 15.20 mPa·s when the viscosity meter range percentage is 60%, which is the best performance. The sample No. 7024 was selected for gel permeation chromatography (GPC) test to determine the molecular weight of 7024. The test results are as follows Figure 2 , Table 2, Table 3.

[0048] Depend on Figure 2 It can be seen that the peak shape is narrow, the high molecular weight is less, the molecular weight distribution is more concentrated, and the polydispersity index is 1.365857.

[0049] Table 2 Molecular weight results of gel chromatography

[0050]

[0051] Table 3 Peak results of gel chromatography

[0052]

[0053] The number average molecular weight is the average molecular weight of all polymer chains, and the weight average molecular weight takes into account that chains with larger molecular weight account for a larger proportion of the total mass, so it can better reflect the influence of high molecular weight chains on all polymer chains. As shown in Table 2, the number average molecular weight of 7024 is 7902 g / mol, and the weight average molecular weight is 10793 g / mol. Since the weight average molecular weight is greater than the number average molecular weight, it means that there are chains with larger molecular weight in the polymer, and these chains account for a larger proportion of the total mass. Therefore, it can be concluded that in the present invention, a polymerization reaction occurs with EDOT as a raw material to obtain a PEDOT polymer.

[0054] Example 2

[0055] Regarding the second embodiment of the present invention, description of parts that are not different from the first embodiment will be omitted and the same reference numerals will be given.

[0056] (1) The method for preparing the electrolyte in Example 2 is the same as that in Example 1.

[0057] (2) Electrode pretreatment:

[0058] Use nickel foam as the counter electrode and glassy carbon as the working electrode. Place the nickel foam electrode in an acetone solution for ultrasonic cleaning for 10 minutes, rinse it with deionized water, place it in a 1 mol / L hydrochloric acid solution for ultrasonic cleaning for 10 minutes, and finally rinse it repeatedly with deionized water and ethanol and dry it. The pretreatment method of the glassy carbon electrode is the same as in Example 1. The current density is set to 15 mA / cm 2, electrochemical polymerization was carried out under stirring conditions, and the reaction time was 2h.

[0059] During the polymerization process, bubbles were observed on the nickel foam electrode, and a small amount of bubbles and blue-black substances were generated on the glassy carbon electrode. The blue-black substances on the glassy carbon electrode were rinsed with ethanol, dried at 55°C for 12 hours, and 0.738 g of the product (7026) was weighed, with a yield of 69%.

[0060] 0.2 g of the product (7026) was taken for gel permeation chromatography (GPC) test to determine the molecular weight of the product. Table 4 shows the molecular weight results of the gel permeation chromatography of the sample of Example 2.

[0061] Table 4 Molecular weight results of gel chromatography

[0062]

[0063] As shown in Table 4, the number average molecular weight of 7026 is 7814 g / mol, and the weight average molecular weight is 10311 g / mol. Since the weight average molecular weight is greater than the number average molecular weight, it indicates that chains with larger molecular weight exist in the polymer, and these chains account for a larger proportion of the total mass. Therefore, it can be concluded that in the present invention, a polymerization reaction occurs using EDOT as a raw material to obtain a PEDOT polymer.

[0064] Example 3

[0065] Regarding the third embodiment of the present invention, description of parts that are not different from the first embodiment will be omitted and the same reference numerals will be given.

[0066] The preparation method of the electrolyte solution in Example 3 is the same as that in Example 1, with nickel foam as the working electrode and platinum sheet as the counter electrode. The pretreatment method of the nickel foam electrode in Example 3 is the same as that in Example 2, and the pretreatment method of the platinum sheet electrode is the same as that in Example 1.

[0067] The current density was set to 15 mA / cm 2 , electrochemical polymerization was carried out under stirring conditions, and the reaction time was 2h.

[0068] During the polymerization process, bubbles were observed to be generated on the platinum electrode and black substances were generated on the nickel foam electrode. The black substances on the nickel foam electrode were washed with ethanol and dried at 55°C for 12 h to obtain 0.621 g of product (7027) with a yield of 58%.

[0069] 0.2 g of the product (7027) was taken for gel permeation chromatography (GPC) test to determine the molecular weight of the product. Table 5 shows the molecular weight results of the gel permeation chromatography of the sample of Example 3.

[0070] Table 5 Molecular weight results of gel chromatography

[0071]

[0072] As shown in Table 5, the number average molecular weight of 7027 is 7401 g / mol, and the weight average molecular weight is 11705 g / mol. Since the weight average molecular weight is greater than the number average molecular weight, it indicates that chains with larger molecular weight exist in the polymer, and these chains account for a larger proportion of the total mass. Therefore, it can be concluded that in the present invention, a polymerization reaction occurs using EDOT as a raw material to obtain a PEDOT polymer.

[0073] Example 4

[0074] Regarding the fourth embodiment of the present invention, description of parts that are not different from those of the first embodiment will be omitted and will be given the same reference numerals.

[0075] The preparation method of the electrolyte solution of Example 4 is the same as that of Example 1. The nickel foam is used as the working electrode. The pretreatment method is the same as that of Example 2. The conductive glass ITO is used as the counter electrode. The electrode is immersed in a sodium hydroxide solution (0.1 mol / L) for about 20 minutes, and repeatedly washed with deionized water until neutral. After washing, it is rinsed with anhydrous ethanol and dried. The current density is set to 15 mA / cm 2 , electrochemical polymerization was carried out under stirring conditions, and the reaction time was 2h.

[0076] During the polymerization process, bubbles and blackening can be observed on the nickel foam electrode, and a layer of uneven black material can be observed on the conductive glass ITO electrode. Under stirring conditions, some black products fall off in the electrolyte. The blue-black material on the glassy carbon electrode was rinsed with ethanol and dried at 55°C for 12 hours to obtain 0.667 g of product (7028), with a yield of 62.3%.

[0077] 0.2 g of the product (7028) was taken for gel permeation chromatography (GPC) test to determine the molecular weight of the product. Table 6 shows the molecular weight results of the gel permeation chromatography of the sample of Example 4.

[0078] Table 6 Molecular weight results of gel chromatography

[0079]

[0080] As shown in Table 6, the number average molecular weight of 7028 is 7501 g / mol, and the weight average molecular weight is 11305 g / mol. Since the weight average molecular weight is greater than the number average molecular weight, it indicates that chains with larger molecular weight exist in the polymer, and these chains account for a larger proportion of the total mass. Therefore, it can be concluded that in the present invention, a polymerization reaction occurs using EDOT as a raw material to obtain a PEDOT polymer.

[0081] Embodiments 5 to 8

[0082] Regarding Embodiments 5 to 8 of the present invention, description of parts that are not different from Embodiment 1 will be omitted and the same reference numerals will be given.

[0083] Only the current density and reaction time in the electrochemical polymerization were changed to obtain the corresponding final product. The gel chromatography molecular weight results of the final product were tested, and the relevant data obtained are shown in Table 7 below.

[0084] Table 7 Electrochemical polymerization reaction and gel chromatography measurement results of Examples 5 to 8

[0085]

[0086] In summary, the synthesis and preparation method of the PEDOT polymer provided by the present invention uses 3,4-ethylenedioxythiophene as a raw material, uses camphorsulfonic acid as a dopant, selects suitable electrodes and pretreatment methods, and performs electrochemical polymerization to obtain the PEDOT polymer. The synthesis process is simple, has a high yield, and can be industrially produced.

[0087] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent changes and modifications made within the scope of the present invention should still fall within the scope of the present invention.

[0088] Comparative Example 1

[0089] The inventors conducted a large number of experiments in the process of obtaining the technical solution of the present invention. Regarding the selection of electrodes, the inventors initially selected conductive glass ITO as the working electrode and platinum sheet electrode as the counter electrode, and conducted experiments after corresponding pretreatment. The details are as follows:

[0090] 1.74 g of camphorsulfonic acid was weighed and dissolved in 75 mL of dimethyl carbonate solution. The mixture was stirred at 40° C. until the camphorsulfonic acid was completely dissolved. Then, 2.13 g of EDOT and 0.134 g of hexamethylphosphoric acid triamide were added.

[0091] Conductive glass ITO was used as the working electrode and platinum electrode as the counter electrode. The conductive glass ITO electrode was immersed in a sodium hydroxide solution (0.1 mol / L) for about 20 minutes, and repeatedly washed with deionized water until neutral. After washing, it was rinsed with anhydrous ethanol and dried. The platinum electrode was ultrasonically cleaned in a 1 mol / L hydrochloric acid solution for 5 minutes, and then repeatedly rinsed with deionized water and ethanol and dried.

[0092] Under stirring conditions, the current density was 15 mA / cm 2 Electrochemical polymerization was carried out with a polymerization time of 2 h. The above electrodes were all pretreated.

[0093] During the polymerization process, it can be observed that there is no obvious phenomenon on the conductive glass ITO electrode, very few bubbles are generated on the platinum electrode, and no film is generated.

[0094] Comparative Example 2

[0095] Regarding Comparative Example 2 of the present invention, description of parts that are the same as those of Comparative Example 1 will be omitted.

[0096] Conductive glass ITO was used as the working electrode, and the counter electrode was replaced with a glassy carbon electrode as the counter electrode, and the treatment method was the same as that in comparative example 1. The treatment method was carried out under stirring conditions with a current density of 15 mA / cm 2 Electrochemical polymerization was carried out with a polymerization time of 2 h. The above electrodes were all pretreated.

[0097] During the polymerization process, it can be observed that there is no obvious phenomenon on the conductive glass ITO electrode and no film is generated on the glassy carbon electrode.

[0098] It can be seen from the above experiments that the selection of electrodes is one of the key points of the present invention. If conductive glass is used as the working electrode, the experiment will fail and the PEDOT polymer cannot be obtained.

Claims

1. A method for synthesizing a PEDOT polymer, characterized in that: The following steps are involved: (1) preparing an electrolyte solution: adding a dopant to a carbonate solution, heating and stirring at 40° C. until the dopant is dissolved, and then adding 3,4-ethylenedioxythiophene and a catalyst to obtain an electrolyte solution; (2) Pre-treat the working electrode and the counter electrode respectively, and then immerse them in the electrolyte solution in (1) at the same time, stir, and electrochemically polymerize to obtain a PEDOT polymer.

2. The method for synthesizing a PEDOT polymer according to claim 1, characterized in that: The carbonate solution in (1) is dimethyl carbonate.

3. The method for synthesizing a PEDOT polymer according to claim 1, characterized in that: The catalyst in (1) is hexamethylphosphoric triamide.

4. The method for synthesizing a PEDOT polymer according to claim 1, characterized in that: The doping agent in (1) is camphorsulfonic acid, and its concentration is 0.1-0.2 mol / L.

5. The method for synthesizing a PEDOT polymer according to claim 1, characterized in that: In the above (1), the concentration of 3,4-ethylenedioxythiophene is 0.1-0.2 mol / L, and the concentration of the catalyst is 0.01-0.5 mol / L.

6. The method for synthesizing a PEDOT polymer according to claim 1, characterized in that: The electrochemical polymerization current density in (2) is 5-15 mA / cm 2 , time is 2-4 h.

7. The method for synthesizing a PEDOT polymer according to claim 1, characterized in that: The working electrode in (2) is selected from any one of platinum sheet, glassy carbon, nickel foam, and cobalt foam; the counter electrode is selected from any one of platinum sheet, glassy carbon, nickel foam, cobalt foam, and conductive glass ITO.

8. The method for synthesizing a PEDOT polymer according to claim 7, characterized in that: The platinum sheet is pretreated by placing it in a 1 mol / L hydrochloric acid solution for ultrasonic cleaning for 5 minutes, then repeatedly rinsing it with deionized water and ethanol, and drying it; The pretreatment method of the glassy carbon as a working electrode is: polishing with 0.05 μm Al2O3 powder, rinsing with deionized water and anhydrous ethanol, and drying; The pretreatment methods of the nickel foam or cobalt foam are: ultrasonic cleaning in an acetone solution for 10 minutes, rinsing with deionized water, ultrasonic cleaning in a 1 mol / L hydrochloric acid solution for 10 minutes, and finally repeatedly rinsing with deionized water and ethanol, and drying; The pretreatment method when the glassy carbon or conductive glass ITO is used as the counter electrode is: immersing the electrode in a 0.1 mol / L sodium hydroxide solution, taking it out after 15-25 minutes, repeatedly washing it with deionized water until it is neutral, rinsing it with anhydrous ethanol after washing, and drying it.

9. The method for synthesizing a PEDOT polymer according to claim 1, characterized in that: The contact areas of the counter electrode and the working electrode with the electrolyte solution are both 10 mm×20 mm, and the volume of the electrolyte solution is 80 mL.

Citation Information

Patent Citations

  • Poly(3,4-ethylenedioxythiophene) aligned array layer thin-film electrode material and preparing method thereof

    CN101587778A

  • Water-soluble poly(3,4-ethylenedioxythiophene) and preparation method for conductive coating thereof

    CN101845136A

  • Poly (3,4-ethylenedioxythiophene) nanowire thin film and synthetic method and application thereof

    CN105887126A

  • Chemical prepn process of nanometer polyethylene thienyl dioxide

    CN1974628A

  • Poly(3,4-ethylenedioxythiophene)

    US20100282998A1