Integrated solid solution electrode and preparation method and application thereof
By regulating the charge distribution and spatial configuration of Ru sites, combining heterogeneous metal elements and solvothermal reaction technology, an integrated solid solution electrode is formed, which solves the durability of Ru-based catalysts under acidic and oxidative conditions, and achieves the full range of Highly efficient OER catalysis and stability improvement in pH range.
Patent Information
- Application Number
- CN202410953513.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing Ru-based OER catalysts have poor durability under acidic and oxidative conditions, and there is still room for improvement in the activity and stability of multi-metal oxides in the full pH range, especially under strong acidic conditions, and most of them are limited in stability. The need for adhesive coating in powder form leads to increased costs and loss of activity.
By synchronously regulating the charge distribution and spatial configuration of Ru sites, heterogeneous metal elements are introduced into Ru oxide to form multi-metal oxides, and solid solution catalysts are grown in situ on the titanium substrate through solvothermal reaction to form an integrated solid solution electrode. Improve the activity and stability of the catalyst.
The good OER catalytic activity and durability of Ru-based catalysts in the entire pH range are achieved, which reduces the amount of precious metals, reduces production costs, and improves the overall stability of the electrode.
Smart Images

Figure CN118910661A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the fields of energy chemical industry and nano material technology, and in particular to an integrated solid solution electrode and a preparation method and application thereof. Background Art
[0002] Since the 20th century, the overuse of fossil energy has led to serious energy crises and environmental problems, which has prompted people to pursue cleaner and more sustainable fuels to replace traditional fossil fuels, such as renewable energy sources such as wind power, solar energy, geothermal energy and biomass energy. Hydrogen has a high energy density (142kJ g -1 ), clean and sustainable development, and is considered one of the important carriers of global energy transformation and development. In recent years, as countries have successively clarified their carbon neutrality timetables, global hydrogen energy has accelerated its development and has become an important tool for energy technology revolution and climate change response in various countries.
[0003] Hydrogen production by water electrolysis is an effective and clean method of producing high-purity hydrogen using renewable energy. Electricity can be obtained through renewable energy sources such as solar energy, hydropower, wind power and nuclear power generation, which can achieve carbon-free and green hydrogen production.
[0004] The electrolytic water splitting reaction is divided into the cathode hydrogen evolution reaction (HER) and the anode oxygen evolution reaction (OER). Since OER involves 4 electron transfers, it is considered to be the rate-determining step. Its slow reaction kinetics limits the overall water splitting efficiency. Therefore, the development of efficient OER catalysts is the key to achieving large-scale water electrolysis hydrogen production. In industrial applications, iridium (Ir)-based materials have good electrocatalytic activity and stability, but the scarcity and extremely high cost of Ir make it difficult to apply them on a large scale in the hydrogen production industry. To date, many transition metal-based OER electrocatalysts have been shown to have good electrocatalytic activity and stability in concentrated alkaline electrolytes (pH>13). However, few electrocatalysts are suitable for use in neutral and low pH media, especially strongly acidic media (pH<1). Most of these catalysts are chemically unstable and are prone to corrosion / decomposition under the highly corrosive and oxidative working conditions of OER. Therefore, the development of non-Ir-based, efficient and stable OER electrocatalysts suitable for OER electrocatalysis under different pH conditions has high technical value and important industrial significance. Summary of the invention
[0005] The present invention is based on the inventor's discovery and understanding of the following facts and problems:
[0006] Since ruthenium (Ru) is more abundant on Earth, its price (about $13.25 / g) is only about one-thirteenth of that of Ir (about $175.34 / g), and Ru-based oxides generally exhibit higher OER activity than Ir-based oxides. Therefore, Ru is considered to be an ideal component element to replace Ir as an OER catalyst. However, Ru oxides are easily over-oxidized and dissolved under acidic and oxidizing conditions, making the durability of Ru-based catalysts poor, which makes the development of Ru-based catalysts with both high activity and stability a huge challenge.
[0007] To address the challenges faced by the above-mentioned Ru-based OER catalysts, the electronic structure of Ru-based electrocatalysts can be optimized by simultaneously regulating the charge distribution and spatial configuration of Ru sites, reducing the adsorption energy barrier of OER intermediates, and inhibiting the dissolution of Ru sites, ultimately achieving a joint improvement in the activity and stability of Ru-based catalysts. By introducing heterogeneous metal elements into Ru oxide to form multi-metal oxides, not only can the amount of Ru be reduced, but also the coordination configuration and charge distribution of Ru sites can be adjusted. However, Ru-based multi-metal oxides face multiple challenges in being used as pH-universal OER catalysts. For example, the choice of stable metal elements under strong acidic conditions is limited (iridium, manganese, titanium, niobium and vanadium, etc.); most multi-metal oxides are prepared by replacing Ru in RuO2 with heterogeneous elements, which makes the bond between Ru and heterogeneous elements weak, weakening the regulatory effect of heterogeneous atoms on the charge distribution and spatial configuration of Ru sites; in addition, most multi-metal oxides are powders and need to be coated on a substrate through a non-conductive binder to prepare a working electrode, which not only increases the preparation cost of the working electrode, but also loses the catalytic activity and stability of the catalyst. Therefore, the OER activity and durability (stability) of Ru-based multi-metal oxides in the entire pH range still need to be improved.
[0008] The present invention aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.
[0009] In one aspect of the present invention, the present invention proposes a method for preparing an integrated solid solution electrode. In some embodiments of the present invention, the method for preparing an integrated solid solution electrode comprises the following steps: dissolving a soluble ruthenium source and a manganese source in water to obtain a precursor solution, or mixing an aqueous solution of a soluble ruthenium source and an aqueous solution of a manganese source to obtain a precursor solution, wherein the manganese source comprises manganate and / or permanganate; placing a titanium substrate and the precursor solution in a reaction vessel, wherein the titanium substrate is located above the precursor solution; heating, so that the raw materials in the reaction vessel undergo a solvothermal reaction to obtain an integrated solid solution electrode, wherein the integrated solid solution electrode comprises a substrate and a solid solution grown on the substrate, wherein the solid solution comprises ruthenium, titanium, manganese and oxygen. Thus, the solid solution catalyst particles in the integrated solid solution electrode prepared by the above method grow directly on the substrate, and the solid solution has a high bonding strength with the substrate, which is beneficial to improving the overall stability of the electrode; the catalyst has good OER catalytic activity and durability in the entire pH range (under acidic, neutral or alkaline conditions).
[0010] In some embodiments of the present invention, the temperature of the solvent thermal reaction is 90° C. to 200° C. and / or the time of the solvent thermal reaction is 1 h to 20 h. This is beneficial to improving the utilization rate of raw materials and the stability of the product.
[0011] In some embodiments of the present invention, a support is placed in the reaction container, and the titanium substrate is placed on the support, so that the titanium substrate is located above the precursor solution; and / or the height difference between the titanium substrate and the liquid surface of the precursor solution is 2 cm to 6 cm. In this way, the solution can be better prevented from contacting the titanium substrate during the reaction process.
[0012] In some embodiments of the present invention, in the precursor solution, the molar ratio of manganese to ruthenium is greater than or equal to 1: 1. This is beneficial to improve the utilization rate of ruthenium in the raw material, thereby improving the catalytic activity of the electrode.
[0013] In some embodiments of the present invention, the soluble ruthenium source includes at least one of ruthenium trichloride hydrate, anhydrous ruthenium trichloride, ammonium chlororuthenate and carbonyl ruthenium chloride; and / or, the manganese source includes at least one of potassium permanganate, sodium permanganate, potassium manganate and sodium manganate; and / or, in the precursor solution, the molar concentration of ruthenium element is 3mmol / L to 15mmol / L.
[0014] In some embodiments of the present invention, the method for preparing an integrated solid solution electrode satisfies at least one of the following conditions: the titanium substrate is titanium foam, titanium felt or titanium mesh; the thickness of the titanium substrate is 0.3 mm to 0.8 mm; the porosity of the titanium substrate is 40% to 70%; before placing the titanium substrate in the reaction container, the titanium substrate is acid-etched; the soluble ruthenium source is ruthenium trichloride hydrate; the manganese source is potassium permanganate; after the solvent thermal reaction, the reaction product is washed and dried to obtain the integrated solid solution electrode.
[0015] In another aspect of the present invention, the present invention proposes an integrated solid solution electrode. In some embodiments of the present invention, the integrated solid solution electrode is prepared by the method described above, and the integrated solid solution electrode includes a substrate and a solid solution on the substrate, the substrate includes metal titanium, and the solid solution includes ruthenium, titanium, manganese and oxygen. As a result, the integrated solid solution electrode has good OER catalytic performance, can be used for OER catalysis under acidic, neutral and alkaline conditions, and has ultra-long durability.
[0016] In some embodiments of the present invention, the solid solution has a face-centered cubic crystal structure, and ruthenium, titanium, and manganese are uniformly dispersed in the solid solution in the form of atoms.
[0017] In some embodiments of the present invention, the integrated solid solution electrode satisfies at least one of the following conditions: the average particle size of the solid solution is 50nm to 400nm; based on the sum of the amounts of metal elements in the solid solution, the molar content of ruthenium is 10% to 80%, the molar content of titanium is 10% to 80%, and the molar content of manganese is 10% to 80%; the area of the integrated solid solution electrode is 1cm 2 ~15cm 2 The integrated solid solution electrode is rectangular, circular, elliptical or irregular in shape, which is conducive to further improving the catalytic activity of the integrated solid solution electrode.
[0018] In another aspect of the present invention, the present invention proposes the use of the aforementioned integrated solid solution electrode in electrocatalysis. The integrated solid solution electrode has good OER catalytic activity, can be used in electrocatalysis, and can maintain good catalytic performance and durability under different pH conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0020] Figure 1A schematic diagram showing an in-situ preparation of an integrated solid solution electrode by a one-step critical gas phase method in one embodiment of the present invention;
[0021] Figure 2 The figure shows the inner lining of the reactor and the brackets of different heights in some embodiments of the present invention;
[0022] Figure 3 The physical pictures showing titanium substrates, brackets and reactor liners of different sizes in some embodiments of the present invention;
[0023] Figure 4 A schematic diagram of in-situ preparation of an integrated solid solution electrode by a one-step critical gas phase method and schematic diagrams of samples of Example 1 and Comparative Example 2 are shown;
[0024] Figure 5 Shows the physical pictures of the samples prepared in Example 1 and Comparative Example 2;
[0025] Figure 6 Shows the physical pictures of the samples prepared in Examples 4 to 6 of the present invention;
[0026] Figure 7 The XRD spectrum, refinement results and crystal structure diagram of the sample in Example 1 of the present invention are shown;
[0027] Figure 8 The TEM image and TEM-Mapping element distribution map of the sample in Example 1 of the present invention are shown;
[0028] Fig. 9 The TEM-EDS spectrum of the sample in Example 1 of the present invention is shown;
[0029] Fig.10 The TEM image and TEM-Mapping element distribution map of the sample in Comparative Example 2 are shown;
[0030] Fig.11 The TEM-EDS spectrum of the sample in Comparative Example 2 is shown;
[0031] Fig.12 The spherical aberration corrected HADDF-STEM image, inverse Fourier transform result and interplanar spacing of the sample in Example 1 are shown;
[0032] Fig.13 Shows Fig.12 The interplanar spacing diagram of the regions corresponding to α and β in Figure b;
[0033] Fig.14 The linear sweep voltammetric curves of the samples of Example 1 and Comparative Examples 1 to 3 in an electrolyte with pH = 0 are shown;
[0034] Fig.15 Shows Fig.14 The corresponding Tafel curve;
[0035] Fig.16 The linear sweep voltammetric curves of the samples of Example 1 and Comparative Examples 1 to 3 in an electrolyte of pH=7 are shown;
[0036] Fig.17 Shows Fig.16 The corresponding Tafel curve;
[0037] Fig.18 The linear sweep voltammetric curves of the samples of Example 1 and Comparative Examples 1 to 3 in an electrolyte of pH=14 are shown;
[0038] Fig.19 Shows Fig.18 The corresponding Tafel curve;
[0039] Fig. 20 Figure a shows the linear sweep voltammetric curves of the samples of Examples 2 to 4 in an electrolyte with pH = 0. Fig. 20 Figure b shows the Tafel curve corresponding to Figure a;
[0040] Fig.21 The voltage-time curves of the samples of Example 1, Comparative Example 1 and Comparative Example 3 in an electrolyte with pH=0 are shown;
[0041] Fig. 22 The voltage-time curves of the samples of Example 1, Comparative Example 1 and Comparative Example 3 in an electrolyte with a pH of 7 are shown;
[0042] Fig.23 The voltage-time curves of the samples of Example 1, Comparative Example 1 and Comparative Example 3 in an electrolyte with pH=14 are shown. DETAILED DESCRIPTION
[0043] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0044] In one aspect of the present invention, the present invention provides a method for preparing an integrated solid solution electrode. In some embodiments of the present invention, the method for preparing an integrated solid solution electrode may include the following steps:
[0045] S100: providing a precursor solution.
[0046] In some embodiments of the present invention, a soluble ruthenium source and a manganese source may be dissolved in water to obtain a precursor solution. In other embodiments of the present invention, an aqueous solution of a soluble ruthenium source and an aqueous solution of a manganese source may be mixed to obtain a precursor solution.
[0047] In some embodiments of the present invention, the soluble ruthenium source may include at least one of ruthenium trichloride hydrate, anhydrous ruthenium trichloride, ammonium chlororuthenate and carbonyl ruthenium chloride. The above ruthenium sources can all be dissolved in water to form a ruthenium-containing solution, which is conducive to the subsequent preparation of a solid solution catalyst by a solvent thermal reaction. In some specific embodiments of the present invention, the soluble ruthenium source may be ruthenium trichloride hydrate, anhydrous ruthenium trichloride, ammonium chlororuthenate or carbonyl ruthenium chloride. In other specific embodiments of the present invention, the soluble ruthenium source may be composed of two or more of ruthenium trichloride hydrate, anhydrous ruthenium trichloride, ammonium chlororuthenate and carbonyl ruthenium chloride, and the specific ratio is not particularly limited in the present invention, and those skilled in the art may set and adjust according to actual needs, as long as a ruthenium-containing solution can be formed.
[0048] In some embodiments of the present invention, the soluble ruthenium source may be ruthenium trichloride hydrate. Ruthenium trichloride hydrate has good solubility, which facilitates the formation of a ruthenium-containing solution. In addition, chloride ions can promote the migration of titanium, which is beneficial to the formation of a titanium-containing solid solution catalyst.
[0049] In some embodiments of the present invention, the molar concentration of ruthenium in the precursor solution may be 3mmol / L to 15mmol / L, for example, the molar concentration of ruthenium may be 3mmol / L, 5mmol / L, 6mmol / L, 8mmol / L, 9mmol / L, 10mmol / L, 12mmol / L, 15mmol / L, etc. Thus, the precursor solution contains an appropriate amount of ruthenium, which can make the solid solution contain a certain amount of ruthenium, thereby facilitating the improvement of the OER catalytic activity of the electrode.
[0050] In some embodiments of the present invention, the manganese source may include manganate and / or permanganate. Manganate or permanganate has strong oxidizing properties and can oxidize ruthenium ions in the solution to form ruthenium tetroxide gas during the subsequent solvothermal reaction.
[0051] In some embodiments of the present invention, the manganese source may include at least one of potassium permanganate, sodium permanganate, potassium manganate and sodium manganate. In some embodiments of the present invention, the manganese source may be potassium permanganate, sodium permanganate, potassium manganate or sodium manganate. In other embodiments of the present invention, the manganese source may be composed of two or more of potassium permanganate, sodium permanganate, potassium manganate and sodium manganate.
[0052] In some specific embodiments of the present invention, the manganese source can be potassium permanganate. In the precursor solution, the concentration of potassium permanganate can be 1 mg / ml to 10 mg / ml. For example, the concentration of potassium permanganate can be 3 mg / ml, 4 mg / ml, 5 mg / ml, 6 mg / ml, 7 mg / ml, etc.
[0053] In some embodiments of the present invention, in the precursor solution, the molar ratio of manganese to ruthenium is greater than or equal to 1:1. Thus, high-valent manganese can completely oxidize ruthenium into ruthenium tetroxide during the reaction, and then form a solid solution catalyst through a critical gas phase reaction. In some embodiments of the present invention, in the precursor solution, the molar ratio of manganese to ruthenium is greater than 1:1, which is conducive to completely oxidizing ruthenium into ruthenium tetroxide, thereby facilitating the utilization rate of ruthenium, and further facilitating the catalytic activity of the solid solution.
[0054] S200: placing a titanium substrate and a precursor solution in a reaction container, with the titanium substrate being located above the precursor solution.
[0055] In some embodiments of the present invention, the reaction container is a reactor having a metal shell and a polytetrafluoroethylene lining. Before the reaction begins, the titanium substrate and the precursor solution are placed in the lining of the reactor. Figure 2 The leftmost container is the reactor liner.
[0056] In the present invention, a titanium substrate is placed above the precursor solution. During the reaction, the titanium substrate does not contact the precursor solution, and the ruthenium tetroxide gas and the manganese-containing gas are in-situ deposited on the surface of the titanium substrate to form a ruthenium titanium manganese oxide solid solution catalyst through a critical gas phase reaction. Figure 1 shown.
[0057] In some embodiments of the present invention, a support can be placed in the reaction vessel, and the titanium substrate can be placed on the support so that the titanium substrate is located above the precursor solution. In some embodiments of the present invention, the support can be made of polytetrafluoroethylene, so that the support can maintain good stability during the solvothermal reaction and will not cause adverse effects on the product.
[0058] In some specific embodiments of the present invention, reference Figure 2 , Figure 2 The three brackets between the middle scale and the reactor liner have different heights. The bracket is wide at the top and narrow at the bottom, and is a hollow structure. When in use, the wider outer wall of the upper part of the bracket fits the inner wall of the reactor liner, and the titanium substrate is placed above the bracket. During the reaction process, the bracket can keep its position fixed, thereby ensuring that the titanium substrate does not contact the solution. Those skilled in the art can also set the specific structure of the bracket according to actual needs, as long as the titanium substrate can be placed above the solution.
[0059] In some embodiments of the present invention, the titanium substrate and the precursor solution are placed in a reaction vessel, so that the height difference between the titanium substrate and the liquid surface of the precursor solution is 2 cm to 6 cm. For example, the height difference between the titanium substrate and the liquid surface of the precursor solution can be 2 cm, 2.5 cm, 3 cm, 4 cm, 4.5 cm, 5 cm, 5.5 cm, 6 cm, etc. The height difference between the titanium substrate and the liquid surface is within the above range, which can well avoid the titanium substrate from contacting the solution during the reaction process, and is conducive to the critical gas phase reaction of manganese-containing vapor and ruthenium tetroxide vapor with the titanium substrate to form a solid solution catalyst. In some specific embodiments, the height difference between the titanium substrate and the liquid surface of the precursor solution can be adjusted to 2 cm to 6 cm by using a bracket.
[0060] In some embodiments of the present invention, the titanium substrate may be titanium foam, titanium felt or titanium mesh. The titanium substrate has a porous structure and a large space, which is conducive to the growth of solid solution particles and material transmission.
[0061] In some embodiments of the present invention, the thickness of the titanium substrate can be 0.3mm to 0.8mm. For example, the thickness of the titanium substrate can be 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.8mm, etc. The above-mentioned titanium substrate has a suitable thickness and good supporting performance, which is convenient for making an integrated electrode.
[0062] In some embodiments of the present invention, the titanium substrate may be foamed titanium, and the thickness of the foamed titanium may be 0.3 mm to 0.8 mm. Thus, the titanium substrate has a relatively large thickness and hardness, and is suitable as a substrate for an integrated electrode.
[0063] In some embodiments of the present invention, the porosity of the titanium substrate can be 40% to 70%. For example, the porosity of the titanium substrate can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, etc. Therefore, the titanium substrate has a rich pore structure, and the three-dimensional skeleton structure can provide a larger space and sufficient sites for the growth of solid solution nanoparticles, and is beneficial to the transmission of substances during the reaction process, promoting rapid reaction.
[0064] In some embodiments of the present invention, the volume ratio of the titanium substrate to the precursor solution may be 1 to 8:10. For example, the volume ratio of the titanium substrate to the precursor solution may be 1:10, 3:10, 4:10, 5:10, 6:10, 8:10, etc.
[0065] In some embodiments of the present invention, the titanium substrate can be rectangular, circular, elliptical or irregular, and titanium substrates of various shapes can be used to prepare integrated solid solution electrodes. In some preferred embodiments, the titanium substrate can be rectangular or circular. In some specific embodiments of the present invention, the titanium substrate can be a square titanium foam, and the size can be adjusted according to the inner diameter of the reactor liner, as shown in FIG. Figure 3 The row adjacent to the titanium base is hollow brackets of different sizes. The size of the upper part of the bracket is consistent with the size of the lower part. The last row is reactor liners of different inner diameters and heights. During the experiment, reactors, brackets and titanium bases of matching sizes can be selected as needed.
[0066] In some embodiments of the present invention, the titanium substrate can be washed first, for example, the titanium substrate can be washed with water, washed with acetone and washed with anhydrous ethanol in sequence. Water washing can remove dust and inorganic impurities on the surface of the titanium substrate, wherein the inorganic impurities may include titanium halides, titanates and / or titanium hydroxides. Acetone washing can remove organic impurities on the surface of the titanium substrate, wherein the organic impurities may include grease. Anhydrous ethanol washing can remove residual acetone on the surface of the titanium substrate, and at the same time, anhydrous ethanol is easy to volatilize and remove. The above washing can remove pollutants on the surface of the titanium substrate, which is conducive to providing uniform sites for the deposition of multi-metal solid solutions.
[0067] In some embodiments of the present invention, the water used for water washing is preferably ultrapure water. In the present invention, the time for water washing, acetone washing and anhydrous ethanol washing can be independently 5 minutes to 15 minutes, for example, the time for water washing, acetone washing and anhydrous ethanol washing can be independently 5 minutes, 8 minutes, 10 minutes, 12 minutes, 15 minutes, etc.
[0068] In the present invention, water washing, acetone washing and anhydrous ethanol washing can be independently performed under ultrasonic conditions, and the ultrasonic power can be 400W to 1000W, for example, the ultrasonic power can be 400W, 600W, 700W, 800W, 1000W, etc. Under the assistance of ultrasound of the above power, it is beneficial to shorten the washing time and to remove impurities on the titanium substrate.
[0069] In the present invention, the amount of water, acetone and anhydrous ethanol used in the washing process is not particularly limited, as long as the titanium substrate can be completely immersed.
[0070] In some embodiments of the present invention, before the titanium substrate is placed in the reaction vessel, the titanium substrate can be acid-etched. This is conducive to the uniform growth of the solid solution, thereby facilitating the uniformity of the reaction product. In some embodiments of the present invention, concentrated hydrochloric acid and water can be mixed in a volume of 1:1, and the titanium substrate can be placed in the mixed solution, and heated at a temperature of 80°C to 120°C (for example, 80°C, 90°C, 100°C, 110°C or 120°C) for 10min to 30min (for example, 10min, 15min, 20min, 25min or 30min) to obtain an acid-etched titanium substrate. In other embodiments of the present invention, the titanium substrate can also be acid-etched using dilute nitric acid, oxalic acid or dilute sulfuric acid.
[0071] S300: heating to make the raw materials in the reaction container undergo a solvothermal reaction to obtain an integrated solid solution electrode.
[0072] In this step, the raw materials in the reaction container are subjected to a solvothermal reaction by heating to obtain an integrated solid solution electrode. In some embodiments of the present invention, the temperature of the solvothermal reaction may be 90°C to 200°C, for example, the temperature of the solvothermal reaction may be 90°C, 100°C, 150°C, 180°C, 200°C, etc. Figure 1 , the reaction is carried out at the above temperature, the high-valent manganese in the raw material can oxidize ruthenium to form ruthenium tetroxide gas, and the manganese source can also form manganese-containing vapor. The ruthenium tetroxide gas, the manganese-containing vapor and the titanium element in the titanium substrate undergo a critical gas phase reaction on the surface of the titanium substrate to generate a ruthenium titanium manganese oxide solid solution, which is in-situ vapor deposited on the titanium substrate to obtain an integrated solid solution electrode in one step.
[0073] In some embodiments of the present invention, reference Figure 1 The integrated solid solution electrode may include a substrate and a solid solution grown on the substrate, wherein the solid solution includes ruthenium, titanium, manganese and oxygen.
[0074] In some embodiments of the present invention, the temperature of the solvothermal reaction can be 90°C to 140°C. For example, the temperature of the solvothermal reaction can be 90°C, 100°C, 110°C, 130°C, 140°C, etc. When the reaction is carried out at the above temperature, the solution is not easy to contact with the titanium substrate, which is conducive to the formation of a ruthenium titanium manganese oxide solid solution. In addition, the above temperature is conducive to the uniform growth of the solid solution particles and the firm bonding of the solid solution particles to the substrate, which is conducive to further improving the catalytic activity and durability of the integrated solid solution electrode.
[0075] In some embodiments of the present invention, the solvent thermal reaction time may be 1 hour to 20 hours, for example, the solvent thermal reaction time may be 1 hour, 5 hours, 10 hours, 15 hours, 20 hours, etc. This is beneficial to improve the utilization rate of the raw materials and allow the raw materials to react fully.
[0076] In some preferred embodiments of the present invention, the solvent thermal reaction time can be 3h to 8h. For example, the solvent thermal reaction time can be 3h, 4h, 5h, 6h, 7h, 8h, etc. Within the above time, the raw materials can be fully reacted, which is beneficial to improve the utilization rate of the raw materials, and is beneficial to shorten the reaction time and save electricity, thereby helping to reduce the preparation cost.
[0077] In some embodiments of the present invention, after the solvothermal reaction, the method for preparing an integrated solid solution electrode may further include the following steps: cooling the solvothermal reaction product, and then performing solid-liquid separation. In the present invention, the temperature of the solvothermal reaction product can be reduced to room temperature, for example, the solvothermal reaction product can be reduced to 10°C to 30°C. In some embodiments, the solvothermal reaction product can be cooled by automatic cooling through a blast drying oven program. In the present invention, there is no special limitation on the method of solid-liquid separation, as long as solid-liquid separation can be achieved.
[0078] In some embodiments of the present invention, the reaction product (solid obtained by solid-liquid separation) can be washed and dried to obtain an integrated solid solution electrode.
[0079] In the present invention, washing the reaction product may include washing with water and washing with anhydrous ethanol in sequence. The number of washing with water and washing with anhydrous ethanol may be 2 to 4 times independently. In some embodiments, the solid product after solid-liquid separation may be washed with water three times, and then washed with anhydrous ethanol three times.
[0080] After washing the solid product, the product can be dried. In some embodiments, the drying temperature can be 40°C to 90°C, and the time can be 2h to 8h. For example, the temperature can be 40°C, 50°C, 55°C, 60°C, 65°C, 70°C, 90°C, etc., and the time can be 2h, 4h, 5h, 6h, 8h, etc. In some embodiments, the product can be vacuum dried.
[0081] In some embodiments of the present invention, reference Figure 4 , part of the titanium substrate is immersed in the precursor solution, and the other part is located above the precursor solution. High-valent manganese oxidizes ruthenium to ruthenium tetroxide, forming ruthenium tetroxide vapor. Ruthenium tetroxide vapor and manganese source vapor undergo critical gas phase reaction on the surface of the titanium substrate above the precursor to form ruthenium titanium manganese oxide solid solution and in-situ vapor deposition on the surface of the titanium substrate; the titanium substrate immersed in the precursor solution can only participate in the liquid phase reaction to form manganese titanium oxide. Figure 4 It can be seen that the morphology of the critical gas phase reaction products is also significantly different from that of the liquid phase reaction products. Figure 5The darker part of the sample is the product of the critical gas phase reaction, and the lighter part is the product of the liquid phase reaction.
[0082] In general, the method for preparing an integrated solid solution electrode proposed in the present invention is simple and convenient for preparing large-area OER electrodes; by carrying out critical gas phase reaction and in-situ gas phase deposition during the solvothermal reaction, an integrated solid solution electrode can be obtained in one step; by forming a ruthenium titanium manganese oxide solid solution, the amount of precious metal ruthenium is greatly reduced, thereby reducing the production cost of the electrode or catalyst; in the integrated solid solution electrode prepared by the preparation method proposed in the present invention, there is a strong electronic interaction between ruthenium, titanium and manganese, and the active center ruthenium is embedded in the face-centered cubic lattice in the form of atoms, which fully exposes the active site and improves the stability of the ruthenium site. The electrode has good OER catalytic performance in a wide pH range (including acidic, neutral and alkaline conditions) and has ultra-long durability.
[0083] In another aspect of the present invention, the present invention proposes an integrated solid solution electrode. In some embodiments of the present invention, the integrated solid solution electrode can be prepared using the method described above, and the integrated solid solution electrode includes a substrate and a solid solution on the substrate, the substrate can include metallic titanium, and the solid solution can include ruthenium, titanium, manganese and oxygen. As a result, there is a strong electronic interaction between ruthenium, titanium and manganese in the solid solution, and the active center ruthenium is embedded in the solid solution lattice in the form of atoms, which fully exposes the active site while regulating the coordination configuration of the ruthenium site, thereby improving the stability of the ruthenium site, so that the solid solution has good electrocatalytic activity and durability.
[0084] In some embodiments of the present invention, the substrate may be titanium foam, titanium felt or titanium mesh.
[0085] In some embodiments, the thickness of the substrate may be 0.3 mm to 0.8 mm, and the porosity may be 40% to 70%.
[0086] In some embodiments of the present invention, reference Figure 1 The solid solution is a face-centered cubic crystal structure, and ruthenium, titanium, and manganese are uniformly dispersed in the solid solution in the form of atoms. As a result, there is a strong electronic interaction between ruthenium, titanium, and manganese. Ruthenium is embedded in the face-centered cubic lattice in the form of atoms, which fully exposes the active sites while regulating the coordination configuration of the ruthenium sites, thereby improving the stability of the ruthenium sites.
[0087] In some embodiments of the present invention, the average particle size of the solid solution can be 50nm to 400nm. For example, the average particle size of the solid solution can be 50nm, 100nm, 200nm, 220nm, 260nm, 280nm, 300nm, 400nm, etc., which is beneficial to increase the specific surface area of the solid solution catalyst. During the water electrolysis reaction, more active sites can be exposed, increasing the reaction rate, which is beneficial to improving the electrocatalytic efficiency of the solid solution.
[0088] In some embodiments of the present invention, based on the sum of the amounts of metal elements in the solid solution, the molar content of ruthenium can be 10% to 80%, the molar content of titanium can be 10% to 80%, and the molar content of manganese can be 10% to 80%. For example, the molar content of ruthenium can be 10%, 20%, 40%, 60%, 80%, etc., the molar content of titanium can be 10%, 30%, 50%, 70%, 80%, etc., and the molar content of manganese can be 10%, 30%, 60%, 80%, etc.
[0089] In some embodiments of the present invention, based on the sum of the amounts of metal elements in the solid solution, the molar content of ruthenium can be 10% to 50%, the molar content of titanium can be 15% to 50%, and the molar content of manganese can be 20% to 65%. For example, the molar content of ruthenium can be 10%, 20%, 25%, 30%, 40%, 50%, etc., the molar content of titanium can be 15%, 25%, 30%, 40%, 45%, 50%, etc., and the molar content of manganese can be 20%, 30%, 40%, 50%, 60%, 65%, etc. This is conducive to further improving the OER catalytic activity and durability of the solid solution catalyst.
[0090] In some embodiments of the present invention, the area of the integrated solid solution electrode may be 1 cm 2 , 3cm 2 , 5cm 2 、10cm 2 、15cm 2 During the preparation process, the area of the electrode can be set or adjusted according to actual needs, and the area of the electrode can be controlled by adjusting the size of the titanium substrate.
[0091] In some embodiments of the present invention, the integrated solid solution electrode may be rectangular, circular, elliptical or irregularly shaped. Figure 6 The black sample is an integrated solid solution electrode. The integrated solid solution electrode can be a square, and the side length of the square can be adjusted according to actual needs.
[0092] In another aspect of the present invention, the present invention proposes the application of the aforementioned integrated solid solution electrode in electrocatalysis. The integrated solid solution electrode has good OER electrocatalytic activity and can be used as an electrode for electrolysis of water to catalyze oxygen evolution reaction in the full pH range. The integrated solid solution electrode has excellent stability and can perform catalytic reactions for thousands of hours.
[0093] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment used are all commercially available. If in the following examples, specific processing conditions and processing methods are not clearly described, then conditions and methods known in the art can be used to process.
[0094] Example 1
[0095] The titanium foam with a thickness of 0.6 mm was cut into a rectangle of 60 mm × 10 mm, and then ultrasonically cleaned with ultrapure water, acetone and anhydrous ethanol for 10 min respectively to obtain clean titanium foam;
[0096] Take 20.0 mg of ruthenium trichloride hydrate and 20.0 mg of potassium permanganate, add 10.0 ml of ultrapure water, and then mix them by ultrasonication at a power of 700 W to obtain a precursor solution;
[0097] Place the cleaned titanium foam and 10 mL of the precursor solution into a 50 mL reactor. Figure 4 As shown, a small part of the titanium foam is immersed in the precursor solution, and the other part is located above the precursor solution and does not contact the precursor solution. The reaction raw materials are heated to perform a solvent thermal reaction at 140°C for 3 hours, and then cooled to 25°C for solid-liquid separation. The solid obtained by solid-liquid separation is washed with ultrapure water 3 times and anhydrous ethanol 3 times in sequence, and the washed solid is dried at a vacuum degree of 85kPa and a temperature of 60°C for 3 hours. The critical gas phase reaction part ( Figure 5 The sample with medium dark color) is the integrated solid solution electrode prepared in Example 1, and the integrated solid solution electrode includes a foam titanium substrate and a ruthenium titanium manganese oxide solid solution grown on the foam titanium substrate.
[0098] Example 2
[0099] An integrated solid solution electrode was prepared in the same manner as in Example 1, except that, in order to obtain only the product of the critical gas phase reaction part, a hollow bracket that fits the inner wall of the reactor liner was designed and manufactured, and the titanium foam was cut into 20 mm × 20 mm squares and placed flat on a bracket with a height of 4.5 cm. After the same solvothermal reaction, an integrated ruthenium titanium manganese oxide solid solution electrode was obtained. During the solvothermal reaction, the titanium foam substrate was not in contact with the solution.
[0100] Example 3
[0101] An integrated solid solution electrode was prepared in the same manner as in Example 2, except that the height of the support was 5.0 cm.
[0102] Example 4
[0103] An integrated solid solution electrode was prepared in the same manner as in Example 2, except that the height of the support was 5.5 cm.
[0104] Example 5
[0105] An integrated solid solution electrode was prepared in the manner of Example 2, except that the specification of the reaction kettle was 100 ml, the size of the titanium foam was 25 mm×25 mm, and the height of the bracket was 5.5 cm.
[0106] Example 6
[0107] An integrated solid solution electrode was prepared in the manner of Example 2, except that the specification of the reaction kettle was 200 ml, the size of the titanium foam was 35 mm×35 mm, and the height of the bracket was 5.5 cm.
[0108] Comparative Example 1
[0109] An integrated solid solution electrode was prepared in the manner of Example 1, except that the titanium foam was replaced with carbon cloth, wherein the solvent thermal critical gas phase reaction product was used as the electrode of Comparative Example 1, which included a carbon cloth substrate and a ruthenium manganese oxide solid solution (RuMnO x )Material.
[0110] Comparative Example 2
[0111] The solvent hot liquid phase reaction part ( Figure 5 The integrated electrode obtained as Comparative Example 2 includes a titanium foam substrate and a titanium manganese oxide solid solution material located on the titanium foam substrate.
[0112] Comparative Example 3
[0113] Mix 325 μL of ethanol, 25 μL of a perfluorinated resin solution (Nafion has a mass content of 5 wt%), 150 μL of ultrapure water, and 20 mg of ruthenium dioxide (purity ≥ 99.99%) to obtain a ruthenium dioxide dispersion;
[0114] 50 μL of ruthenium dioxide dispersion was added dropwise onto the surface of a square titanium foam with a thickness of 0.6 mm and a size of 10 mm×10 mm, and dried at 60° C. for 6 h to obtain a ruthenium dioxide / titanium foam electrode.
[0115] The synthesis schematic diagram of the samples of Example 1 and Comparative Example 2 is as follows Figure 4 As shown, the material obtained from the critical gas phase reaction part of the solvent thermal reaction is the sample of Example 1, and the material obtained from the liquid phase reaction part is the sample of Comparative Example 2. Figure 5 , the sample of Example 1 is darker in color, while the sample of Comparative Example 2 is lighter in color. During the reaction, since all ruthenium ions are oxidized to ruthenium tetroxide gas, and react with potassium permanganate vapor on the surface of the titanium substrate to form a ruthenium titanium manganese oxide solid solution, the sample of Example 1 presents a dark color of ruthenium oxide, while the liquid phase is a titanium manganese oxide solid solution formed by the reaction of potassium permanganate solution with the titanium substrate, so the sample of Comparative Example 2 presents a light color of titanium manganese oxide.
[0116] In order to obtain only the product of the critical gas phase reaction part, the inventor designed and manufactured hollow brackets of different heights that fit the inner wall of the reactor liner to determine the optimal area of the critical gas phase reaction part. Figure 2 and Figure 3 After confirming the optimal height of the critical gas phase reaction, refer to Figure 3 and Figure 6 The present invention prepares a large-area integrated solid solution electrode by enlarging the size of the titanium substrate, the reactor and the bracket. The integrated solid solution electrodes of Examples 4 to 6 are shown in the figure below. Figure 6 As shown, it can be seen that the products of Examples 4 to 6 all exhibit the dark color of ruthenium oxide.
[0117] The integrated solid solution material prepared in Example 1 was subjected to XRD detection to obtain an XRD spectrum, as shown in FIG. Figure 7 The obtained XRD data were refined by Rietveld to obtain the accurate crystal structure of the ruthenium titanium manganese oxide solid solution, which is a face-centered cubic structure with a space group of Fm-3m and a molar ratio of ruthenium, titanium and manganese of 0.24:0.29:0.47.
[0118] The integrated ruthenium titanium manganese oxide solid solution material prepared in Example 1 and the sample prepared in Comparative Example 2 were examined by transmission electron microscopy to obtain TEM images. Figure 8 TEM image of the sample of Example 1 and the corresponding distribution of ruthenium, titanium and manganese elements, Fig. 9 TEM-EDS elemental analysis diagram of the sample in Example 1, Figure 8 and Fig. 9 It can be seen that the ruthenium, titanium and manganese elements are uniformly distributed in the integrated ruthenium titanium manganese oxide solid solution material prepared by the critical gas phase reaction in the solvothermal reaction of the present invention. Fig.10 TEM image of the sample of Comparative Example 2 and the corresponding distribution of titanium, manganese and oxygen elements, Fig.11 TEM-EDS element analysis of the sample of Comparative Example 2. Fig.10 and Fig.11 It can be seen that there is no ruthenium element in the integrated titanium manganese oxide solid solution material prepared by the critical liquid phase reaction in the solvothermal reaction. The above results prove that all the ruthenium ions in ruthenium trichloride are oxidized by potassium permanganate to ruthenium tetroxide gas, which reacts with potassium permanganate vapor and titanium substrate in the critical gas phase to generate a uniform ruthenium titanium manganese oxide solid solution material and is in-situ deposited on the titanium substrate.
[0119] The integrated ruthenium titanium manganese oxide solid solution material prepared in Example 1 was subjected to spherical aberration-corrected transmission electron microscopy detection to obtain a HADDF-STEM image, as shown in FIG. Fig.12 shown. Fig.12 Figure a is the HADDF-STEM image of the sample in Example 1, in which the bright spots are metal atoms. In order to show the atomic arrangement more clearly, Figure a is subjected to inverse Fourier transformation to obtain a higher resolution image. Fig.12 Figure b; To further analyze the intensity distribution and interplanar spacing of each atomic site, select Fig.12 The line intensity analysis of the α and β atomic columns in Figure b is as follows: Fig.13 As shown. Fig.12 and Fig.13 It can be seen that the integrated ruthenium titanium manganese oxide solid solution material provided by the present invention belongs to the cubic crystal system, and the interplanar spacing is 0.23nm, which corresponds to the (020) crystal plane of the ruthenium titanium manganese oxide solid solution material, and is consistent with the XRD test results; and the ruthenium, titanium and manganese elements are evenly distributed. Figures 7 to 9 and Figures 12-13 It can be seen that the critical gas phase method proposed in the present invention successfully prepared an integrated and uniform ruthenium titanium manganese oxide solid solution material, in which ruthenium, titanium, manganese and oxygen elements are fully mixed in the form of single atoms and highly dispersed in the face-centered cubic crystal structure.
[0120] Next, the application of the integrated ruthenium titanium manganese oxide solid solution material provided by the present invention in electrocatalytic water decomposition in a wide pH range is described.
[0121] Electrocatalytic activity test: 0.5M sulfuric acid aqueous solution (pH=0), 0.5M PBS buffer solution (pH=7) and 1.0M potassium hydroxide aqueous solution (pH=14) were used as electrolytes, and a typical three-electrode configuration (a platinum sheet was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and the electrodes of Examples 1 to 4 and Comparative Examples 1 to 3 were used as working electrodes) was used to perform an electrochemical activity test using an electrochemical workstation. The voltammetric characteristic curve was obtained at a scan rate of 2mV / s as shown in FIG. Fig.14 (pH = 0), Fig.16 (pH = 7) and Fig.18 (pH = 14). Fig.14 , Fig.16 and Fig.18 The Tafel curves of various voltammetric characteristic curves are calculated by linear sweep voltammetric curves. The results are shown in Fig.15 , Fig.17 and Fig.19 As shown. Figures 14 to 19 It can be seen that the integrated ruthenium titanium manganese oxide solid solution material provided by the present invention can be directly used as an anode to perform electrocatalytic water decomposition in a wide pH range. Fig.14 , the sample of Example 1 is at pH = 0, 10mAcm -2 The lowest overpotential at the current density of is only 165.3mV (overpotential = voltage value obtained by test in the figure - theoretical voltage value 1.23V), which is 13.8mV, 277.0mV and 58.7mV lower than the lowest overpotential of comparative examples 1 to 3, respectively; Fig.16 , the sample of Example 1 is at pH = 7, 10mAcm -2 The lowest overpotential at the current density of 2.547 W was only 234.1 mV, which was 22.2 mV, 320.0 mV and 101.3 mV lower than the lowest overpotential of Comparative Examples 1 to 3, respectively; Fig.18 , the sample of Example 1 was at pH = 14, 10 mA cm -2 The lowest overpotential at the current density of 1.5 is only 185.9 mV, which is 25.2 mV, 347.6 mV and 53.7 mV lower than the lowest overpotential of Comparative Examples 1 to 3, respectively. Fig.15 , Fig.17 and Fig.19 Using the integrated solid solution material of Example 1 of the present invention as an electrode, the Tafel slopes at pH = 0, pH = 7, and pH = 14 are only 48.4 mV dec, respectively. -1 、49.1mV dec -1 and 38.0mV dec -1 , indicating that the integrated solid solution material provided by the present invention has excellent electrode reaction kinetics and a high electrocatalytic reaction rate.
[0122] Fig. 20 The effectiveness of the critical gas phase method provided by the present invention in preparing the integrated solid solution material is confirmed. The integrated solid solution material generated by the critical gas phase reaction at the height of 4.5 cm, 5.0 cm and 5.5 cm as an electrode can reach 10 mA cm under the condition of pH = 0. -2 The overpotentials were 172.7 mV, 186.6 mV, and 176.3 mV at current densities of 1.3, 1.7, and 1.6 mV, respectively, and the Tafel slopes were 49.2 mV dec. -1 、49.1mV dec -1 and 46.8mV dec -1 The above test results prove that the critical gas phase reaction in the solvothermal reaction process can generate an integrated ruthenium titanium manganese oxide solid solution, and exhibit excellent electrochemical activity in the electrocatalytic oxygen evolution reaction. The optimal gas phase reaction height is 5.5 cm from the titanium substrate to the bottom of the reactor inner lining.
[0123] Electrocatalytic stability test: 0.5 M sulfuric acid aqueous solution (pH = 0), 0.5 M PBS buffer solution (pH = 7) and 1.0 M potassium hydroxide aqueous solution (pH = 14) were used as electrolytes, respectively, and a typical three-electrode configuration was adopted (a platinum sheet was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and the samples of Example 1, Comparative Example 1 and Comparative Example 3 were used as working electrodes). The test area was 1 × 1 cm 2 , select the "chronopotentiometry" method, set the current value to 10mA, then the current density is 10mAcm -2 , the overpotential-time curve is obtained as Figures 21 to 23 As shown. Figures 21 to 23 It can be seen that under the conditions of pH = 0, pH = 7 and pH = 14, the integrated ruthenium titanium manganese oxide solid solution electrode provided by the present invention can continue electrolysis for 3000h, 1500h and 2000h, respectively. The stable time is 1000 times, 300 times and 200 times longer than that of the commercial ruthenium dioxide sample (Comparative Example 3), respectively, proving that the integrated ruthenium titanium manganese oxide solid solution material provided by the present invention has excellent electrocatalytic stability.
[0124] In the description of the present invention, the orientation or position relationship indicated by the terms "upper" and "lower" etc. is based on the orientation or position relationship shown in the drawings and is only for the convenience of describing the present invention rather than requiring the present invention to be constructed and operated in a specific orientation. Therefore, it should not be understood as a limitation on the present invention.
[0125] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "some specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.
[0126] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing an integrated solid solution electrode, characterized in that: The following steps are involved: Dissolving a soluble ruthenium source and a manganese source in water to obtain a precursor solution, or mixing an aqueous solution of a soluble ruthenium source and an aqueous solution of a manganese source to obtain a precursor solution, wherein the manganese source comprises manganate and / or permanganate; placing a titanium substrate and the precursor solution in a reaction container, wherein the titanium substrate is located above the precursor solution; The raw materials in the reaction container are heated to undergo a solvothermal reaction to obtain an integrated solid solution electrode, wherein the integrated solid solution electrode comprises a substrate and a solid solution grown on the substrate, wherein the solid solution comprises ruthenium, titanium, manganese and oxygen.
2. The method according to claim 1, characterized in that The temperature of the solvent thermal reaction is 90°C to 200°C; And / or, the solvent thermal reaction time is 1 h to 20 h.
3. The method according to claim 1, characterized in that placing a support in the reaction container, and placing the titanium substrate on the support so that the titanium substrate is located above the precursor solution; And / or, the height difference between the titanium substrate and the liquid surface of the precursor solution is 2 cm to 6 cm.
4. The method according to claim 1, characterized in that In the precursor solution, the molar ratio of manganese element to ruthenium element is greater than or equal to 1:
1.
5. The method according to any one of claims 1 to 4, characterized in that: The soluble ruthenium source includes at least one of ruthenium trichloride hydrate, anhydrous ruthenium trichloride, ammonium chlororuthenate and carbonyl ruthenium chloride; and / or, the manganese source comprises at least one of potassium permanganate, sodium permanganate, potassium manganate and sodium manganate; And / or, in the precursor solution, the molar concentration of ruthenium element is 3 mmol / L to 15 mmol / L.
6. The method according to any one of claims 1 to 4, characterized in that: At least one of the following conditions is met: The titanium substrate is titanium foam, titanium felt or titanium mesh; The thickness of the titanium substrate is 0.3 mm to 0.8 mm; The porosity of the titanium substrate is 40% to 70%; Before placing the titanium substrate in the reaction container, performing acid etching on the titanium substrate; The soluble ruthenium source is ruthenium trichloride hydrate; The manganese source is potassium permanganate; After the solvothermal reaction, the reaction product is washed and dried to obtain the integrated solid solution electrode.
7. An integrated solid solution electrode, characterized in that: The integrated solid solution electrode is prepared by the method described in any one of claims 1 to 6, and the integrated solid solution electrode includes a substrate and a solid solution on the substrate, the substrate includes metallic titanium, and the solid solution includes ruthenium, titanium, manganese and oxygen.
8. The integrated solid solution electrode according to claim 7, characterized in that: The solid solution has a face-centered cubic crystal structure, and ruthenium, titanium and manganese are uniformly dispersed in the solid solution in the form of atoms.
9. The integrated solid solution electrode according to claim 7 or 8, characterized in that: At least one of the following conditions is met: The average particle size of the solid solution is 50nm to 400nm; Based on the sum of the amounts of the metal elements in the solid solution, the molar content of the ruthenium element is 10% to 80%, the molar content of the titanium element is 10% to 80%, and the molar content of the manganese element is 10% to 80%; The area of the integrated solid solution electrode is 1 cm 2 ~15cm 2 ; The integrated solid solution electrode is rectangular, circular, elliptical or irregular in shape.
10. Use of the integrated solid solution electrode according to any one of claims 7 to 9 in electrocatalysis.