Vanadium ion doped copper oxide / cuprous oxide / foamy copper electrode material and preparation method thereof

Through vanadium ion-doped copper oxide/cubous oxide/foam copper composite nanorod array electrode materials, the problem of scarcity and limited performance of existing lithium-ion batteries and other low-cost batteries in energy storage devices is solved, and high The specific capacitor and good rate performance are suitable as the negative electrode material for supercapacitors, and the preparation method is simple and low-cost.

CN119008258APending Publication Date: 2024-11-22BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411214833.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing lithium-ion batteries and other low-cost ion batteries have scarce resources, high costs, low charge and discharge rates and safety problems in energy storage devices, which limits their wide application, and the performance of existing negative electrode materials is limited, hindering hybrid capacitors. development.

Method used

Copper oxide/cubous oxide/foam copper foam composite nanorod array electrode material is used to dopant vanadium ion, and the copper hydroxide nanorod array is grown in situ at room temperature by chemical oxidation, combined with the reduction-nucleation mechanism at low temperature hydrothermal conditions The porous structure is formed under the formation of a porous structure to improve the conductivity and electrochemical properties of the material.

Benefits of technology

It has achieved high specific capacitance value and good rate performance, and the material's conductivity and electrochemical performance have been significantly improved. It is suitable as a negative electrode material for supercapacitors. It has a simple preparation method and is cheap, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005021291000000011
    Figure HDA0005021291000000011
  • Figure HDA0005021291000000012
    Figure HDA0005021291000000012
  • Figure HDA0005021291000000013
    Figure HDA0005021291000000013
Patent Text Reader

Abstract

The invention provides a nanorod array electrode material formed by a vanadium ion doped copper oxide / cuprous oxide / foamy copper substrate and a preparation method thereof. The nanorod array electrode material has an expression of V-CuO / Cu2O / CF. The preparation method comprises the following steps: firstly, carrying out chemical oxidation treatment on foamy copper to obtain a copper hydroxide nanorod array precursor, and then carrying out hydrothermal treatment on the precursor by adopting NaBH4 and NH4VO3 to obtain a final material which is a nanorod array structure formed by stacking nanoparticles and has abundant mesopores and micropores. The radius of tetravalent vanadium ions obtained by reduction of NaBH4 in the hydrothermal process is similar to that of copper ions, so that the tetravalent vanadium ions can exist by isometrically replacing part of copper sites. The method is simple to operate and low in raw material cost, the utilization rate of the foamy copper is increased, and a reaction product is green and pollution-free. The specific capacitance value of the product is 65-120F / cm < 2 >, and the rate capability is 60-80%. Therefore, the material is expected to be widely used in electrode materials of energy storage devices such as supercapacitors and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrode material preparation, and in particular to vanadium ion-doped copper oxide / cuprous oxide / copper foam electrode materials and preparation methods thereof. The materials are suitable for use as electrode materials for energy storage devices such as supercapacitors. Background Art

[0002] Nowadays, with the increasing consumption of fossil resources, the problem of global warming has attracted people's attention, so it is particularly important to seek renewable clean energy. The problem that follows is that the demand for economical, efficient, long-term and safe storage of clean energy has become increasingly urgent.

[0003] Among the existing energy storage devices, lithium-ion batteries are the typical representatives of ion batteries, which occupy a huge market share in energy storage devices. However, the further application of lithium-ion batteries is currently facing some limitations, which are due to the uneven distribution of lithium resources on the earth, high cost, scarcity (only 0.0017wt.%) and other reasons. In addition, compared with aqueous hybrid capacitors, other low-cost ion batteries, such as sodium-ion batteries and potassium-ion batteries, have problems that cannot be ignored, such as low charge and discharge rates and worrying safety. Therefore, aqueous hybrid capacitors are the most competitive candidates for ion batteries, which can achieve the goals of high energy density, power density and satisfactory safety by combining battery-type electrode materials. In terms of energy storage mechanism, battery-type electrode materials achieve the purpose of storing a large amount of charge by undergoing a reversible redox reaction with electrolyte ions. However, limited high-performance negative electrode materials have hindered the widespread application of hybrid capacitors to a certain extent. Therefore, finding a negative electrode material with excellent performance and matching with high-performance positive electrode materials is a hot topic of research.

[0004] At present, low-cost, naturally abundant transition metal oxides and sulfides with multiple oxidation states as main features have been studied in depth by researchers as battery-type electrode materials. Among them, copper-based materials have unique electronic structure characteristics, low cost, environmental friendliness and high capacity, and are currently considered to be the most promising negative electrode materials in hybrid capacitors.

[0005] For example, the document Journal of Alloys and Compounds, 2019, 782, 1103-1113 reported a heteroatom-doped carbon / copper oxide / cuprous oxide composite electrode material, which was first calcined at 600°C for two hours, and then the obtained carbon material was treated with acid to remove the residual metal oxides, and finally subjected to a hydrothermal treatment step to form copper oxide / cuprous oxide on the surface of the carbon material. The negative electrode material exhibits a specific capacitance of 147F / g, and can maintain 93% of its capacity after 10,000 cycles. Although this preparation method is convenient for large-scale preparation of heteroatom-doped carbon materials, the electrode capacity formed after further loading transition metal oxides is relatively low, and high temperature and high pressure are required, which increases the energy consumption of production, and the overall steps are cumbersome and the performance is limited. The document Inorganic Chemistry Frontiers, 2023, 10, 6369-6383 proposes a CuCo2S x (OH) y The specific steps of heterogeneous negative electrode materials are as follows: first, a copper-cobalt precursor is generated by a hydrothermal reaction at 120°C for 6 hours on a nickel foam substrate, and then a copper-cobalt composite sulfide is obtained by a further hydrothermal sulfurization reaction at 120°C for 12 hours. On this basis, a further step of electrodeposition is performed to convert it into the final electrode material. The final material still maintains the flower ball morphology of the precursor, and many nanoparticles are formed on the nanosheets that make up the flower ball, which is beneficial to increase the electrochemical active specific surface area of ​​the material. As a negative electrode material, it can be used at 5mA / cm 2 The current density is 2.94F / cm 2 However, this preparation method has too many steps, and repeated hydrothermal treatment can easily affect the mechanical stability of the nickel foam substrate.

[0006] Research in recent years has shown that doping metal cations into the main material can regulate its electronic structure, improve the conductivity of the material, and thus improve its electrochemical performance. For example, the literature ACS Nano, 2024, 18, 3, 2149-2161 reported a molybdenum disulfide electrode material rich in sulfur vacancies with ethylene molecular intercalation and cobalt doping (Co-EG / S V -MoS2), where ethylene molecular intercalation can expand the interlayer spacing of molybdenum disulfide materials, and cobalt doping occupies some molybdenum sites to further promote electron transmission, thereby activating the substrate surface. Carbon fiber cloth was added to a reaction solution composed of ammonium molybdate, thiourea, cobalt nitrate and ethylene glycol, and Co-EG / S was obtained after a one-step hydrothermal reaction at 200°C for 24 hours. V -MoS2 material. This material is at 1mA / cm 2 The current density is 1884.36mF / cm 2The area specific capacitance is eight times higher than that of the original MoS2 electrode material. When the current density is increased to 20 mA / cm 2 The disadvantage of this preparation method is that the active loading of the material obtained after 24 hours of high temperature reaction is relatively low, only 1.5 mg / cm 2 , resulting in low synthesis efficiency, which is not conducive to expanding scale production.

[0007] In recent years, due to the high abundance of vanadium on earth, its multiple valence states, and its ionic radius being similar to that of common transition metal ions that make up electrode materials, the idea of ​​using it to dope and modify the electronic structure of transition metal host materials has attracted more and more attention from researchers. For example, the literature ACS Nano, 2017, 11, 11574-11583 obtained vanadium-doped NiS2 materials by a two-step method. First, nickel-vanadium layered double hydroxides were obtained after hydrothermal reaction at 120°C for 12 hours, and then vanadium-doped NiS2 materials were obtained after 200 minutes of sulfur vapor sulfidation in a tube furnace at 400°C under a hydrogen / argon atmosphere. This work adopted the idea of ​​post-treating the vanadium-containing precursor to introduce vanadium into the host material, but it involved a high-temperature mixed atmosphere calcination step, which increased energy consumption and experimental costs.

[0008] The preparation method adopted in this patent is simple to operate, has low requirements for reaction conditions and reaction equipment, is short in time, and does not require additional addition of other copper salts, which greatly improves the utilization rate of low-cost foam copper, reduces dead volume, and the reaction product is green and pollution-free. The method is also convenient for large-scale production. In this preparation method, cheap foam copper is used as both the copper source and the substrate material. After obtaining the copper hydroxide nanorod array precursor through a simple chemical oxidation step at room temperature, a relatively low temperature hydrothermal treatment is performed to simultaneously achieve the two purposes of cation doping and phase change. The active loading capacity of the in-situ generated tetravalent vanadium ion-doped copper oxide / cuprous oxide on the foam copper is high, which is 12.8 mg / cm 2 , and the material has excellent area specific capacitance and can be used as the negative electrode material of aqueous hybrid capacitors. Summary of the invention

[0009] The purpose of the present invention is to provide a nanorod array electrode material consisting of a vanadium ion-doped copper oxide / cuprous oxide / foam copper substrate and a preparation method thereof, wherein the material is suitable for use as an electrode material for energy storage devices such as supercapacitors.

[0010] The technical scheme of the present invention is that after treating the foamed copper with a chemical oxidation solution, a copper hydroxide nanorod array precursor is obtained in situ, which is used as a copper source and self-supporting substrate for subsequent treatment; further based on the reduction-nucleation mechanism, the copper hydroxide precursor is hydrothermally treated in a reaction solution composed of a strong reducing agent NaBH4 and a vanadium source NH4VO3. During the reaction, pentavalent vanadium is reduced to tetravalent vanadium by excess NaBH4. Since the radius of tetravalent vanadium ions and copper ions is similar, it is easy to isomorphously replace part of the copper sites and remain in the corresponding copper species, and copper hydroxide is also reduced to cuprous oxide and cupric oxide, and gas is generated during the reaction, forming abundant mesopores in the nanorod structure, thereby obtaining a porous tetravalent vanadium ion-doped copper oxide / cuprous oxide / foamed copper composite nanorod array electrode material. By modifying the metal oxide material with cationic sulfur, the conductivity of the metal oxide can be improved and its specific capacitance value can be increased.

[0011] The present invention provides a vanadium ion-doped copper oxide / cuprous oxide / foam copper composite electrode material, the chemical formula of which is V-CuO / Cu2O / CF, and the microstructure of which is composed of porous nanorod-like materials with a diameter in the range of 220-700nm, wherein the nanorods are formed by stacking many tiny nanoparticles and forming many pores, so that the material is in the mesoporous range; the specific capacitance value of the electrode material is 65-120F / cm 2 , the rate performance is between 60% and 80%.

[0012] The preparation method of the V-CuO / Cu2O / CF electrode material provided by the present invention comprises the following specific steps:

[0013] A. Wash the orange copper foam with anhydrous ethanol for 5-10 minutes, then wash it with 3-6% dilute hydrochloric acid solution for 5-10 minutes, take it out and rinse it with deionized water for later use;

[0014] B. Prepare a clear NaOH solution with a concentration range of 2.0-2.5M, add (NH4)2S2O8 in an amount of 0.02-0.03 g (NH4)2S2O8 per ml of NaOH solution, and stir ultrasonically for 1-3 min to dissolve to obtain a fresh solution for chemical oxidation of copper foam;

[0015] C. The immersion area per ml of the above reaction solution is 0.12-0.32 cm 2 Add copper foam in a ratio of 1:1 to 2:1, react for 15-25 minutes, take out the electrode material, rinse it with deionized water, rinse it with anhydrous ethanol, put it in a blast dryer at 60-65°C for 3-6 hours, and obtain a copper hydroxide nanorod array material;

[0016] D. Dissolve NH4VO3 in a water bath at 80-90°C to prepare a solution with a concentration range of 0.0005-0.0025M. After 5-10 minutes, naturally cool the clear yellowish solution, add NaBH4 thereto to form a solution with a concentration range of 0.0125-0.025M, stir ultrasonically for 2-5 minutes to dissolve, transfer the brown reaction solution to the lining of a hydrothermal reactor, add the copper hydroxide nanorod array electrode sheet obtained in step C, and hydrothermally react at 125-140°C for 3-6 hours. After natural cooling, take out and wash with deionized water, and dry in a blower dryer at 60-65°C for 5-7 hours to obtain the final vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material. Its microstructure is composed of porous nanorod-like materials with a diameter range of 220-700nm. The nanorods are composed of many tiny nanoparticles piled up and forming rich pores, making the material in the mesoporous range; the specific capacitance value of the electrode material is 65-120F / cm 2 , the rate performance is between 60% and 80%.

[0017] The invention is characterized in that a simple chemical oxidation method is used to treat low-cost foam copper to obtain a precursor of a copper hydroxide nanorod array morphology, so that the precursor can be used as a copper source and a substrate in subsequent reactions; the precursor is hydrothermally treated with a strong reducing agent NaBH4 using a reduction-nucleation mechanism, and the material after the reaction exhibits a nanorod array structure formed by the accumulation of nanoparticles; since the added NH4VO3 (V) is reduced to tetravalent vanadium ions by excessive NaBH4, it is easy to isomorphously replace part of the copper sites and dope them into the copper species, and the corresponding copper hydroxide precursor is also reduced to cuprous oxide and cupric oxide; the gas generated during the reaction can form abundant mesopores in the nanorod structure, thereby obtaining a porous tetravalent vanadium ion-doped copper oxide / cuprous oxide / foam copper composite nanorod array electrode material.

[0018] The obtained V-CuO / Cu2O / CF material was characterized and its application performance tested. The results are shown in Figure 1-8

[0019] Figure 1 This is a scanning electron microscope (SEM) characterization of the V-CuO / Cu2O / CF material prepared in Example 1 and the corresponding diameter distribution statistical result diagram. It can be seen from the figure that it is a nanorod-like material composed of nanoparticle stacking, and its average diameter is 352.28nm.

[0020] Figure 2 This is the X-ray diffraction (XRD) characterization of the V-CuO / Cu2O / CF material prepared in Example 1. As can be seen from the figure, relevant diffraction peaks of CuO and Cu2O appear respectively, indicating that the material is V-CuO / Cu2O / CF material.

[0021] Figure 3 This is the transmission electron microscopy (TEM) characterization of the V-CuO / Cu2O / CF material prepared in Example 1. As can be seen from the figure, the V-CuO / Cu2O / CF material has a rod-like structure.

[0022] Figure 4 This is a scanning electron microscope (SEM) characterization of the V-CuO / Cu2O / CF material prepared in Example 2 and the corresponding diameter distribution statistical result diagram. It can be seen from the figure that it is a nanowire material with an average diameter of 220.34nm.

[0023] Figure 5 This is the scanning electron microscope (SEM) characterization of the V-CuO / Cu2O / CF material prepared in Example 4. As can be seen from the figure, it is a nanowire material with an average diameter of 692.32 nm.

[0024] Figure 6 This is the cyclic voltammetry curve of the V-CuO / Cu2O / CF electrode prepared in Example 1 in 1 mol / L KOH electrolyte. As can be seen from the figure, there are obvious redox characteristic peaks, and the curve shape at each scanning speed remains consistent, which shows that the material has good reversibility.

[0025] Figure 7 The charge and discharge curves of the V-CuO / Cu2O / CF electrode prepared in Example 1 at different current densities in 1 mol / L KOH electrolyte. 2 、30mA / cm 2 , 50mA / cm 2 , 70mA / cm 2 and 100mA / cm 2 When the specific capacitance is 107.30F / cm 2 (29.81mAh / cm 2 ), 106.86F / cm 2 (29.68mAh / cm 2 ), 113.95F / cm 2 (31.65mAh / cm 2 ), 106.47F / cm 2 (29.58mAh / cm 2 ) and 76.3F / cm 2 (21.19mAh / cm 2 ), and the results show that the material has excellent specific capacitance.

[0026] Figure 8The charge-discharge rate curve of the V-CuO / Cu2O / CF electrode prepared in Example 1 in 1 mol / L KOH electrolyte. It can be seen from the figure that with the increase of current density, the specific capacitance value decreases. 2 Increase to 100mA / cm 2 , the specific capacitance value dropped to 71.1% of the initial value, indicating that the electrode material still has a relatively ideal specific capacitance value under high charge and discharge rate conditions, which shows that the synergistic effect of the composite structure improves the electrochemical performance of the material.

[0027] Beneficial effects of the present invention:

[0028] (1) The present invention makes full use of inexpensive copper foam as both a copper source and a substrate, and chemically oxidizes and in-situ grows copper hydroxide nanorod arrays on the copper foam at room temperature; on this basis, a tetravalent vanadium ion-doped copper oxide / cuprous oxide / copper foam electrode material is obtained by further hydrothermal reaction with NH4VO3 and NaBH4.

[0029] (2) According to the results of UV-visible diffuse reflectance spectroscopy, the electronic structure of CuO / Cu2O was optimized, the band gap of the material was reduced, and the conductivity of the material was increased after partial doping with vanadium ions to replace the copper sites. The first-principles calculation results show that vanadium doping increases the electron cloud density near the copper sites and promotes the charge transfer efficiency, indicating that more charges will be involved in the electrochemical process, promoting the interaction between the material and OH - The redox reaction between the two species is reduced, and the adsorption energy of OH- on the electrode is also reduced, which helps to improve the overall electrochemical performance of the material.

[0030] (3) The prepared V-CuO / Cu2O / CF material has good supercapacitor negative electrode performance, with a specific capacitance value of 65-120F / cm 2 , the rate performance is 60%-80%. Therefore, it is expected to be widely used as anode material in supercapacitors and even other energy storage devices.

[0031] (4) The preparation method adopted by the present invention is simple to operate, has low requirements on reaction conditions and reaction equipment, takes a short preparation time, and does not require additional supplementation of other copper salts, which greatly improves the utilization rate of low-cost foam copper and reduces dead volume. The product obtained by the reaction is green and pollution-free. The method is also convenient for large-scale production, which fully reflects the concept of low-carbon economy and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the scanning electron microscope (SEM) characterization of V-CuO / Cu2O / CF prepared in Example 1.

[0033] Figure 2This is the X-ray diffraction (XRD) characterization of V-CuO / Cu2O / CF prepared in Example 1.

[0034] Figure 3 This is the transmission electron microscopy (TEM) characterization of V-CuO / Cu2O / CF prepared in Example 1.

[0035] Figure 4 This is the scanning electron microscope (SEM) characterization of V-CuO / Cu2O / CF prepared in Example 2.

[0036] Figure 5 This is the scanning electron microscope (SEM) characterization of V-CuO / Cu2O / CF prepared in Example 4.

[0037] Figure 6 This is the cyclic voltammetry curve of the V-CuO / Cu2O / CF electrode prepared in Example 1.

[0038] Figure 7 1 is the charge and discharge curve of the V-CuO / Cu2O / CF electrode prepared in Example 1 at different current densities.

[0039] Figure 8 This is the charge and discharge rate curve of the V-CuO / Cu2O / CF electrode prepared in Example 1. DETAILED DESCRIPTION

[0040] Example 1

[0041] A. Wash the orange copper foam with anhydrous ethanol for 10 minutes, then with 5% diluted hydrochloric acid solution for 5 minutes, take it out and rinse it with deionized water for later use;

[0042] B. Prepare a clear NaOH solution with a concentration of 2.5M, add (NH4)2S2O8 at a rate of 0.023 g (NH4)2S2O8 per ml of NaOH solution, and stir ultrasonically for 2 min to dissolve to obtain a fresh solution for chemical oxidation of copper foam;

[0043] C. The immersion area per ml of the above reaction solution is 0.24 cm 2 Add copper foam in a ratio of 1:1 to 1:1, react for 20 min, take out the electrode material, rinse with deionized water, rinse with anhydrous ethanol, and dry in a blast dryer at 60°C for 3 h to obtain a copper hydroxide nanorod array material;

[0044] D. Dissolve NH4VO3 in a water bath at 85°C to make a 0.0015M solution. After 10 minutes, cool the clear yellowish solution naturally, add NaBH4 to form a 0.025M solution, stir ultrasonically for 2 minutes to dissolve, transfer the brown reaction solution to the lining of the hydrothermal reactor, add the copper hydroxide nanorod array electrode sheet obtained in step C, and hydrothermally react at 130°C for 4 hours. After cooling naturally, take out and wash with deionized water, and dry in a blast dryer at 60°C for 7 hours to obtain the final vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material. Its microstructure is composed of porous nanorod-like materials with an average diameter of 352.28nm. The nanorods are composed of many tiny nanoparticles stacked together to form abundant pores, so that the material is in the mesoporous range; the specific capacitance value of the electrode material is 107.3F / cm 2 , the rate performance is 71.1%.

[0045] The electrochemical performance of the obtained V-CuO / Cu2O / CF was tested:

[0046] In the three-electrode test system, the electrode material was used as the working electrode in a 1 mol / L KOH electrolyte and in the -1-0 V (vs Hg / HgO) voltage window to perform cyclic voltammetry, charge-discharge, and charge-discharge rate tests. The results are shown in Figure 6-8 .

[0047] Example 2

[0048] A. Wash the orange copper foam with anhydrous ethanol for 8 minutes, then with 4.5% diluted hydrochloric acid solution for 6 minutes, and then rinse with deionized water for later use;

[0049] B. Prepare a clear NaOH solution with a concentration of 2.5M, add (NH4)2S2O8 at a feed rate of 0.028 g (NH4)2S2O8 per ml of NaOH solution, and stir ultrasonically for 2 minutes to dissolve to obtain a fresh solution for chemical oxidation of copper foam;

[0050] C. The immersion area per ml of the above reaction solution is 0.24 cm 2 Add copper foam in a ratio of 1:1 to 1:1, react for 20 min, take out the electrode material, rinse with deionized water, rinse with anhydrous ethanol, and dry in a blast dryer at 60°C for 3 h to obtain a copper hydroxide nanorod array material;

[0051] D. Dissolve NH4VO3 in a water bath at 85°C to make a 0.0005M solution. After 10 minutes, cool the clear yellowish solution naturally, add NaBH4 to form a 0.025M solution, stir ultrasonically for 2 minutes to dissolve, transfer the brown reaction solution to the lining of the hydrothermal reactor, add the copper hydroxide nanorod array electrode sheet obtained in step C, and hydrothermally react at 130°C for 4 hours. After cooling naturally, take out and wash with deionized water, and dry in a blast dryer at 60°C for 7 hours to obtain the final vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material. Its microstructure is composed of porous nanorod-like materials with an average diameter of 220.34nm. The nanorods are composed of many tiny nanoparticles stacked together to form abundant pores, making the material in the mesoporous range; the specific capacitance value of the electrode material is 67.6F / cm 2 , the rate performance is 63.1%.

[0052] Example 3

[0053] A. Wash the orange copper foam with anhydrous ethanol for 10 minutes, then with 4.5% diluted hydrochloric acid solution for 5 minutes, and then rinse with deionized water for later use;

[0054] B. Prepare a clear NaOH solution with a concentration of 2.25M, add (NH4)2S2O8 at a feed rate of 0.023 g (NH4)2S2O8 per ml of NaOH solution, and stir ultrasonically for 1 min to dissolve to obtain a fresh solution for chemical oxidation of copper foam;

[0055] C. The immersion area per ml of the above reaction solution is 0.32 cm 2 Add copper foam in a ratio of 1:1 to 1:1, react for 23 minutes, take out the electrode material, rinse it with deionized water, rinse it with anhydrous ethanol, and dry it in a blast dryer at 62°C for 4 hours to obtain a copper hydroxide nanorod array material;

[0056] D. Dissolve NH4VO3 in a water bath at 85°C to make a 0.0015M solution. After 8 minutes, cool the clear yellowish solution naturally, add NaBH4 to form a 0.02M solution, stir ultrasonically for 3 minutes to dissolve, transfer the brown reaction solution to the lining of the hydrothermal reactor, add the copper hydroxide nanorod array electrode sheet obtained in step C, and hydrothermally react at 128°C for 4 hours. After cooling naturally, take out and wash with deionized water, and dry in a blast dryer at 60°C for 6 hours to obtain the final vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material. Its microstructure is composed of porous nanorod-like materials with an average diameter of 402.86nm. The nanorods are composed of many tiny nanoparticles stacked together to form abundant pores, making the material in the mesoporous range; the specific capacitance value of the electrode material is 87.5F / cm 2 , the rate performance is 78.4%.

[0057] Example 4

[0058] A. Wash the orange copper foam with anhydrous ethanol for 10 minutes by ultrasonic, then wash it with 5% diluted hydrochloric acid solution for 10 minutes by ultrasonic, take it out and rinse it with deionized water for later use;

[0059] B. Prepare a clear NaOH solution with a concentration of 2.5M, add (NH4)2S2O8 at a rate of 0.023 g (NH4)2S2O8 per ml of NaOH solution, and stir ultrasonically for 2 min to dissolve to obtain a fresh solution for chemical oxidation of copper foam;

[0060] C. The immersion area per ml of the above reaction solution is 0.18 cm 2 Add copper foam in a ratio of 1:1 to 1:1, react for 25 min, take out the electrode material, rinse with deionized water, rinse with anhydrous ethanol, and dry in a blast dryer at 65 °C for 5 h to obtain a copper hydroxide nanorod array material;

[0061] D. Dissolve NH4VO3 in a water bath at 85°C to make a 0.0025M solution. After 10 minutes, cool the clear yellowish solution naturally, add NaBH4 to form a 0.025M solution, stir ultrasonically for 5 minutes to dissolve, transfer the brown reaction solution to the lining of the hydrothermal reactor, add the copper hydroxide nanorod array electrode sheet obtained in step C, and hydrothermally react at 130°C for 4 hours. After cooling naturally, take out and wash with deionized water, and dry in a blast dryer at 65°C for 6 hours to obtain the final vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material. Its microstructure is composed of porous nanorod-like materials with an average diameter of 692.32nm. The nanorods are composed of many tiny nanoparticles stacked together to form abundant pores, so that the material is in the mesoporous range; the specific capacitance value of the electrode material is 57.6F / cm 2 , the rate performance is 65.6%.

[0062] Example 5

[0063] A. Wash the orange copper foam with anhydrous ethanol for 10 minutes, then with 5% diluted hydrochloric acid solution for 5 minutes, take it out and rinse it with deionized water for later use;

[0064] B. Prepare a clear NaOH solution with a concentration of 2.3M, add (NH4)2S2O8 at a rate of 0.03 g (NH4)2S2O8 per ml of NaOH solution, and stir ultrasonically for 3 min to dissolve to obtain a fresh solution for chemical oxidation of copper foam;

[0065] C. The immersion area per ml of the above reaction solution is 0.24 cm 2 Add copper foam in a ratio of 1:1 to 1:1, react for 23 minutes, take out the electrode material, rinse it with deionized water, rinse it with anhydrous ethanol, put it in a blast dryer and dry it at 60°C for 6 hours to obtain a copper hydroxide nanorod array material;

[0066] D. Dissolve NH4VO3 in a water bath at 90°C to make a 0.0015M solution. After 10 minutes, cool the clear yellowish solution naturally, add NaBH4 to form a 0.0125M solution, stir ultrasonically for 3 minutes to dissolve, transfer the brown reaction solution to the lining of the hydrothermal reactor, add the copper hydroxide nanorod array electrode sheet obtained in step C, and hydrothermally react at 135°C for 4 hours. After cooling naturally, take out and wash with deionized water, and dry in a blast dryer at 60°C for 7 hours to obtain the final vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material. Its microstructure is composed of porous nanorod-like materials with an average diameter of 276.5nm. The nanorods are composed of many tiny nanoparticles stacked together to form abundant pores, making the material in the mesoporous range; the specific capacitance value of the electrode material is 91.2F / cm 2 , the rate performance is 61.3%.

Claims

1. A method for preparing a vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material, characterized in that Prepare according to the following specific steps: A. Wash the orange copper foam with anhydrous ethanol for 5-10 minutes, then wash it with 3-6% dilute hydrochloric acid solution for 5-10 minutes, take it out and rinse it with deionized water for later use; B. Prepare a clear NaOH solution with a concentration range of 2.0-2.5M, add (NH4)2S2O8 in an amount of 0.02-0.03 g (NH4)2S2O8 per ml of NaOH solution, and stir ultrasonically for 1-3 min to dissolve to obtain a fresh solution for chemical oxidation of copper foam; C. The immersion area of ​​the above copper foam solution is 0.12-0.32cm per ml. 2 Add copper foam in a ratio of 1:1 to 2:1, react for 15-25 minutes, take out the electrode material, rinse it with deionized water, rinse it with anhydrous ethanol, put it in a blast dryer at 60-65°C for 3-6 hours, and obtain a copper hydroxide nanorod array material; D. Dissolve NH4VO3 in a water bath at 80-90°C to prepare a solution with a concentration range of 0.0005-0.0025M. After 5-10 minutes, cool the clear yellowish solution naturally, add NaBH4 to form a solution with a concentration range of 0.0125-0.025M, stir ultrasonically for 2-5 minutes to dissolve, transfer the brown reaction solution to the lining of a hydrothermal reactor, add the copper hydroxide nanorod array electrode sheet obtained in step C, and perform hydrothermal reaction at 125-140°C for 3-6 hours. After natural cooling, take out and wash with deionized water, and dry in a blower dryer at 60-65°C for 5-7 hours to obtain the final vanadium ion-doped copper oxide / cuprous oxide / foam copper electrode material, the chemical formula of which is: V-CuO / Cu2O / CF.

2. A vanadium ion-doped copper oxide / cuprous oxide / copper foam electrode material prepared by the method of claim 1.